MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Commercial Bronze, UNS C22000 (90-10 Bronze), OSO35 Temper rod
Categories: Metal; Nonferrous Metal; Copper Alloy; Bronze

Material Notes: Good to excellent corrosion resistance. Excellent cold workability, good hot workability for blanking, coining, drawing, piercing and punching, shearing, spinning, squeezing and swaging, stamping heading and upsetting, roll threading and knurling, hot forging and pressing.

Applications: etching bronze, grillwork, screen cloth, weather-stripping, lipstick cases, compacts, marine hardware, screws, and rivets.

Test specimen: rod - 12.7mm diameter.

Key Words: CDA 220, CZ101, ISO CuZn10, CEN CW501L, Gilding metal, 90/10 brass, corrosion resistant, cold workable, hot workable
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.80 g/cc0.318 lb/in³
Grain Size  3.0 µm
@Treatment Temp. 370 °C
3.0 µm
@Treatment Temp. 698 °F
cold drawn to a 37% reduction in area then annealed 1h; grain size before annealing was 0.05mm
 9.0 µm
@Treatment Temp. 400 °C
9.0 µm
@Treatment Temp. 752 °F
cold drawn to a 37% reduction in area then annealed 1h; grain size before annealing was 0.05mm
 23 µm
@Treatment Temp. 500 °C
23 µm
@Treatment Temp. 932 °F
cold drawn to a 37% reduction in area then annealed 1h; grain size before annealing was 0.05mm
 32 µm
@Treatment Temp. 600 °C
32 µm
@Treatment Temp. 1110 °F
cold drawn to a 37% reduction in area then annealed 1h; grain size before annealing was 0.05mm
 47 µm
@Treatment Temp. 690 °C
47 µm
@Treatment Temp. 1270 °F
cold drawn to a 37% reduction in area then annealed 1h; grain size before annealing was 0.05mm
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 5555
Tensile Strength, Ultimate 275 MPa39900 psi
 245 MPa
@Treatment Temp. 700 °C
35500 psi
@Treatment Temp. 1290 °F
cold drawn to a 37% reduction in area then annealed 1h
 260 MPa
@Treatment Temp. 600 °C
37700 psi
@Treatment Temp. 1110 °F
cold drawn to a 37% reduction in area then annealed 1h
 280 MPa
@Treatment Temp. 500 °C
40600 psi
@Treatment Temp. 932 °F
cold drawn to a 37% reduction in area then annealed 1h
 335 MPa
@Treatment Temp. 400 °C
48600 psi
@Treatment Temp. 752 °F
cold drawn to a 37% reduction in area then annealed 1h
 405 MPa
@Treatment Temp. 300 °C
58700 psi
@Treatment Temp. 572 °F
cold drawn to a 37% reduction in area then annealed 1h
 450 MPa
@Treatment Temp. 15.0 °C
65300 psi
@Treatment Temp. 59.0 °F
cold drawn to a 37% reduction in area then annealed 1h
 450 MPa
@Treatment Temp. 100 °C
65300 psi
@Treatment Temp. 212 °F
cold drawn to a 37% reduction in area then annealed 1h
 450 MPa
@Treatment Temp. 200 °C
65300 psi
@Treatment Temp. 392 °F
cold drawn to a 37% reduction in area then annealed 1h
Elongation at Break 50 %50 %In 50 mm
Modulus of Elasticity 115 GPa16700 ksi
Poissons Ratio 0.3070.307
Machinability 20 %20 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 44.0 GPa6380 ksi
Shear Strength 220 MPa31900 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.00000272 ohm-cm
@Temperature 1100 °C
0.00000272 ohm-cm
@Temperature 2010 °F
liquid phase
 0.00000391 ohm-cm
@Temperature 20.0 °C
0.00000391 ohm-cm
@Temperature 68.0 °F
Magnetic Susceptibility -1.00e-6 - -8.60e-8-1.00e-6 - -8.60e-8cgs units
 
Thermal PropertiesMetricEnglishComments
CTE, linear 18.4 µm/m-°C
@Temperature 20.0 - 300 °C
10.2 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.376 J/g-°C0.0899 BTU/lb-°F
Thermal Conductivity 189 W/m-K
@Temperature 20.0 °C
1310 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 1020 - 1045 °C1870 - 1913 °F
Solidus 1020 °C1870 °F
Liquidus 1045 °C1913 °F
Boiling Point 1400 °C
@Pressure 0.101 MPa
2550 °F
@Pressure 14.6 psi
Approximate
Annealing Point 427 - 788 °C800 - 1450 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 425 - 800 °C797 - 1470 °F
Hot-Working Temperature 750 - 875 °C1380 - 1610 °F
Recrystallization Temperature 370 °C698 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 89 - 91 %89 - 91 %
Iron, Fe <= 0.050 %<= 0.050 %
Lead, Pb <= 0.050 %<= 0.050 %
Zinc, Zn 10 %10 %
 
Descriptive Properties
Velocity of Sound3720 m/sat 20°C

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Phosphor bronze 8% Sn, UNS C52100, H02 Temper rod
Phosphor bronze 5% Sn, UNS C51000, H02 Temper 25 mm rod
Low-silicon bronze B, UNS C65100, OSO35 Temper rod
Commercial Bronze, UNS C22000 (90-10 Bronze), H00 Temper rod
Aluminum Bronze, UNS C61300, O60 Temper

MC22000c4 / 10999

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.