MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Mitsui AURUM® PL450C Polyimide
Categories: Polymer; Thermoplastic; Polyimide, Thermoplastic; Thermoplastic Polyimide, Unfilled

Material Notes: AURUM PL450C is a high performance thermoplastic polyimide for precision injection molded components and extruded products. A member of the AURUM family of advanced engineering resins, unfilled AURUM PL450C offers a unique balance of mechanical and thermal properties for superior performance in demanding automotive, business machinery, industrial equipment, aerospace, and semiconductor equipment applications. AURUM exhibits outstanding resistance to chemicals and radiation, a low coefficient of thermal expansion, ultrahigh purity, low outgassing in a vacuum, excellent electrical properties, and flame resistance. AURUM PL450C can be conventionally extruded to produce high performance wire & cable insulation, thin-wall tubing, and fiber.

Applications: AURUM PL450C injection molded components are excellent replacements for metals, ceramics, and other plastics. High performance AURUM PL450C parts include heat-resistant gears, seals, ferrules and other fasteners, coil bobbins, semiconductor manufacturing and handling equipment components, and thermal and electrical insulators. Products produced from extruded AURUM PL450C resin include thin-wall tubing, wire and cable insulation, monofilament, and rod stock shapes.

Information provided by DuPont

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.33 g/ccASTM D792
Water Absorption 0.34 %24 hrs @ 73°F; ASTM D570
Moisture Absorption at Equilibrium 0.24 %73°F; 60 RH, 24hrs
Linear Mold Shrinkage 0.0083 cm/cmASTM D955
Melt Flow 4.5 - 7.5 g/10 min
@Load 1.05 kg,
Temperature 400 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 13370 psiASTM D638
 8400 psi
@Temperature 149 °C
ASTM D638
Elongation at Yield 90 %ASTM D638
 90 %
@Temperature 149 °C
ASTM D638
Modulus of Elasticity 400 ksiASTM D882
Flexural Strength 19900 psiASTM D790
 12800 psi
@Temperature 149 °C
ASTM D790
Flexural Modulus 426.8 ksiASTM D790
 369.9 ksi
@Temperature 149 °C
ASTM D790
Compressive Strength 11100 psi
@Temperature 149 °C
JIS K7208
 17360 psi
@Temperature 22.8 °C
JIS K7208
Izod Impact, Notched 1.70 ft-lb/inASTM D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+17 - 1.00e+18 ohm-cmASTM D257
Surface Resistance 1.00e+17 - 1.00e+18 ohmASTM D257
Dielectric Constant 3.1
@Frequency 1e+6 Hz
ASTM D150
 3.2
@Frequency 1000 Hz
ASTM D150
Dissipation Factor 0.00090
@Frequency 1000 Hz
ASTM D150
 0.0034
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesOriginal ValueComments
CTE, linear 30.0 µin/in-°F
@Temperature 22.8 °C
MD; ASTM D696
 30.0 µin/in-°F
@Temperature 73.0 °C
TD; ASTM D696
Specific Heat Capacity 0.240 BTU/lb-°FDSC
 1.004 J/g-°C
@Temperature 100 °C
DSC
 1.423 J/g-°C
@Temperature 300 °C
DSC
Thermal Conductivity 0.174333 W/m-KASTM C177
Melting Point 388 °CDSC
Deflection Temperature at 0.46 MPa (66 psi) 238 °CASTM D648
Glass Transition Temp, Tg 250 °CDSC
Flammability, UL94 V-0
@Thickness 0.400 mm
 5VA
@Thickness 2.00 mm
Oxygen Index 47 %
@Thickness 3.20 mm
ASTM D2863

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Mitsui AURUM® JCN3030 Polyimide, Carbon Fiber Filled
Mitsui AURUM® JGN6230 Thermoplastic Polyimide Resin, Crystalline
Solvay CYCOM® 2237 Polyimide Resin System
Mitsui AURUM® JGN3030 Polyimide, Glass Fiber Filled
Mitsui AURUM® JCQ3025 Thermoplastic Polyimide Resin, Wear/Friction Grade

PMIT045E / 53226

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.