MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Lubrizol Telene 1650 A/BK Dicyclopentadiene (DCPD)
Categories: Polymer; Thermoset; Polydicyclopentadiene (PDCPD)

Material Notes: Telene® is a two-component system based on extra-high purity dicyclopentadiene (DCPD). Telene® is processed using a standard high-pressure RIM Equipment (Reaction Injection Molding). Telene® results in a polymer showing a unique combination of stiffness and high impact resistance, as well as good thermal properties. Telene® is self-demolding without any need for release agents.

Information provided by Noveon, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.03 g/ccASTM D 792
Brookfield Viscosity 310 - 390 cP
@Temperature 30.0 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 114ASTM D 785
Tensile Strength, Yield 43.0 MPaISO 527
Elongation at Yield 5.0 %ISO 527
Tensile Modulus 1.87 GPaISO 527
Flexural Strength 67.0 MPaISO 1783
Flexural Modulus 1.85 GPaISO 178
Izod Impact, Notched (ISO) 30.0 kJ/m²ASTM D 256
 
Thermal PropertiesOriginal ValueComments
CTE, linear 90.0 µm/m-°C
@Temperature 20.0 °C
ASTM D 696
Maximum Service Temperature, Air >= 180 °CExotherm Temp; Method 4
Deflection Temperature at 1.8 MPa (264 psi) 120 °CASTM D 648
Glass Transition Temp, Tg 155 °CMethod 1
Smoke Density 1.33 - 1.66 minAt 30°C; Method 4
 
Processing PropertiesOriginal ValueComments
Processing Temperature 60.0 °Cnon show side
 80.0 °Cshow side

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Lubrizol Telene 1620 A/BK Dicyclopentadiene (DCPD)
Lubrizol Telene 1610 A/B & A/BK Dicyclopentadiene (DCPD)
Overview of materials for Polydicyclopentadiene (PDCPD)
Metton LMR M1534 Liquid Molding Resin
Metton LMR M1539 Liquid Molding Resin

PNOVE01 / 55262

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.