MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Trinseo MAGNUM™ 375 HH Acrylonitrile Butadiene Styrene (ABS) Resin
Categories: Polymer; Thermoplastic; ABS Polymer

Material Notes: Overview: High Heat, Low Gloss, Medium Impact ABS resin for injection molding

Applications:

  • Automotive interior trim applications requiring low volatile organic compounds (VOC)
Automotive Specifications:
  • CHRYSLER MS-DB-191
  • CHRYSLER MS-DB-300
  • VAG VW-TL 527
  • VAG VW-TL 527 B
  • VAG VW-TL 527 A

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.06 g/cc0.0383 lb/in³ASTM D792; ISO 1183/B
Linear Mold Shrinkage, Flow 0.0057 cm/cm0.0057 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.0056 cm/cm0.0056 in/inASTM D955
Melt Flow 2.1 g/10 min
@Load 3.80 kg,
Temperature 230 °C
2.1 g/10 min
@Load 8.38 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 47.0 MPa6820 psiISO 527-2
 49.0 MPa7110 psi51 mm/min; ASTM D638
Elongation at Break 3.5 %3.5 %ISO 527-2/50
 8.8 %8.8 %51 mm/min; ASTM D638
Elongation at Yield 2.9 %2.9 %ISO 527-2/50
 3.1 %3.1 %51 mm/min; ASTM D638
Tensile Modulus 2.30 GPa334 ksi51 mm/min; ASTM D638
 2.33 GPa338 ksiISO 527-2
Flexural Strength 71.7 MPa10400 psi3-point, 2 mm/min; ISO 178
 76.5 MPa11100 psiMethod I (3 point load), 1.3 mm/min; ASTM D790
Flexural Modulus 2.30 GPa334 ksi3-point, 2 mm/min; ISO 178
 2.41 GPa350 ksiMethod I (3 point load), 1.3 mm/min; ASTM D790
Izod Impact, Notched  1.30 J/cm
@Temperature -30.0 °C
2.44 ft-lb/in
@Temperature -22.0 °F
ASTM D256
 2.20 J/cm
@Temperature 23.0 °C
4.12 ft-lb/in
@Temperature 73.4 °F
ASTM D256
Izod Impact, Notched (ISO)  10.0 kJ/m²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
ISO 180/A
 16.0 kJ/m²
@Temperature 23.0 °C
7.61 ft-lb/in²
@Temperature 73.4 °F
ISO 180/A
Charpy Impact, Notched  1.10 J/cm²
@Temperature -30.0 °C
5.23 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 2.20 J/cm²
@Temperature 23.0 °C
10.5 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
Dart Drop, Total Energy  23.0 J
@Temperature -30.0 °C
17.0 ft-lb
@Temperature -22.0 °F
Peak Energy; ASTM D3763
 30.1 J
@Temperature 23.0 °C
22.2 ft-lb
@Temperature 73.4 °F
Peak Energy; ASTM D3763
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 77.0 µm/m-°C
@Temperature -40.0 - 100 °C
42.8 µin/in-°F
@Temperature -40.0 - 212 °F
ASTM E831
CTE, linear, Transverse to Flow 95.0 µm/m-°C
@Temperature -40.0 - 100 °C
52.8 µin/in-°F
@Temperature -40.0 - 212 °F
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 98.0 °C208 °FUnannealed; ISO 75-2/B
 99.4 °C211 °FUnannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 81.7 °C179 °FUnannealed; ASTM D648
 84.0 °C183 °FUnannealed; ISO 75-2/A
Vicat Softening Point 105 °C
@Load 5.10 kg
221 °F
@Load 11.2 lb
Rate A (50°C/h); ISO 306/B50; ASTM D1525
Flame Spread 30.0 mm/min1.18 in/minFMVSS 302
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 238 °C460 °F
Middle Barrel Temperature 249 °C480 °F
Front Barrel Temperature 254 °C489 °F
Nozzle Temperature 249 - 254 °C480 - 489 °F
Melt Temperature 243 - 271 °C469 - 520 °F
Mold Temperature 38.0 - 66.0 °C100 - 151 °F
Drying Temperature 82.0 - 85.0 °C180 - 185 °F
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Trinseo MAGNUM™ 375 HP Acrylonitrile Butadiene Styrene (ABS) Resin
MetalTek MTEK 375 Aluminum Bronze
Polymer Resources ABS-GP-HH General Purpose ABS, High Heat
Parker Chomerics CHO-SEAL 1310 Conductive Elastomer
Omni Plastics OmniTech™ ABS 24 HH ABS

PZZDWST076 / 142285

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.