MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
INEOS Styrolution Lustran® 248BS Acrylonitrile Butadiene Styrene (ABS)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Molded

Material Notes: Lustran® 248BS is a high-gloss, medium-impact injection molding resin that has been specially formulated for excellent surface lubricity using internal additives. Healthcare certifications, Medium impact toughness, High gloss, Excellent surface lubricity. Applications: Components of intravenous (IV) systems, Surgical instruments, Diagnostic test kits

Information provided by Styrolution.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.05 g/ccASTM D 792
Linear Mold Shrinkage 0.0040 - 0.0060 cm/cmASTM D 955
Melt Flow 6.0 g/10 min
@Load 3.80 kg,
Temperature 230 °C
ASTM D 1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 110ASTM D 785
Tensile Strength, Yield 42.1 MPaASTM D 638
Tensile Modulus 2620 MPaASTM D 638
Flexural Strength 72.4 MPaASTM D 790
Flexural Modulus 2690 MPaASTM D 790
Izod Impact, Notched 5.00 ft-lb/in
@Temperature 23.0 °C
ASTM D 256
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 87.8 °Cunannealed; ASTM D 648
 
Processing PropertiesOriginal ValueComments
Melt Temperature 218 - 260 °C
Mold Temperature 29.0 - 60.0 °C
Drying Temperature 79.0 °C
@Time 7200 - 14400 sec

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSTYR9848 / 216075

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.