MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

Sika Sikaflex® Construction Sealant One-component, all purpose, polyurethane sealant
Categories: Polymer; Thermoset; Polyurethane, TS; Thermoset Polyurethane, Elastomer, Unreinforced

Material Notes: Sikaflex Construction Sealant is a premium grade, moisture-cured, 1-component, polyurethane based, non-sag elastomeric sealant. Meets Federal specification TT-S-00230C, Type II, Class A. Meets ASTM C-920, Type S, Grade NS, Class 35, use T, NT, O, M, G, I; Canadian standard CAN/CGSB 19.13-M87.

Where to Use:

  • Designed for all types of joints where maximum depth of sealant will not exceed 1/2 in.
  • Suitable for vertical or horizontal joints; readily placeable at 40°F (4°C).
  • Has many applications as an elastic sealant between materials with dissimilar coefficients of expansion.
  • Ideal for:
    • Weatherproofing of joints between brickwork, blockwork, masonry, wood and concrete or metal frames
    • Joints in walls, floors, balconies, around window or door frames
    • Expansion joints
    • Roofing
Advantages:
  • High elasticity – cures to a tough, durable, flexible consistency with exceptional cut and tear resistance.
  • Stress relaxation.
  • Excellent adhesion – bonds to most construction materials without a primer.
  • Excellent resistance to aging, weathering.
  • Non-staining.
  • Urethane-based; suggested by EPA for radon reduction.
  • Paintable with water-, oil- and rubber-based paints.
  • Capable of ±35% joint movement.

Information provided by Sika Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Volatile Organic Compounds (VOC) Content 40 g/l40 g/l
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 35 - 4535 - 4521 day; ASTM C661
Tensile Strength 1.21 MPa175 psi21 day; ASTM D412
Tensile Stress at Strain 0.241 MPa
@Strain 25 %
35.0 psi
@Strain 25 %
21 day; ASTM D412
Elongation at Break 550 %550 %21 day; ASTM D412
50% Modulus 0.414 MPa
@Strain 50 %
0.414 MPa
@Strain 50 %
21 day; ASTM D412
100% Modulus 0.586 MPa
@Strain 100 %
85.0 psi
@Strain 100 %
21 day; ASTM D412
Tear Strength 9.64 kN/m55.0 pliASTM D624
Peel Strength 3.51 kN/m20.0 pliConcrete, 0% Adhesion loss; TT-S-00230C, ASTM C-794
 3.51 kN/m20.0 pliAluminum, 0% Adhesion loss; TT-S-00230C, ASTM C-794
 3.51 kN/m20.0 pliGlass, 0% Adhesion loss; TT-S-00230C, ASTM C-794
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 76.7 °C170 °F
Minimum Service Temperature, Air -40.0 °C-40.0 °F
 
Processing PropertiesMetricEnglishComments
Cure Time 180 min3.00 hourTo touch
 5760 - 10100 min96.0 - 168 hourFinal cure
Tack-Free Time 180 - 300 min3.00 - 5.00 hour
Shelf Life 12.0 Month
@Temperature 4.00 - 35.0 °C
12.0 Month
@Temperature 39.2 - 95.0 °F
in original unopened cartridge
 
Descriptive Properties
ColorsWhite, Limestone, Capitol Tan, Dark Bronze, and Medium Bronze

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
A. Schulman DuraGrip™ DGR 6030 NC/BK Thermoplastic Elastomer (TPE)
Sika Sikaflex® -11 FC One part advanced polyurethane, elastomeric sealant/adhesive
Resinlab® UR3010 Black Polyurethane Potting System
Dow Isoplast® 151 Polyurethane (PUR-RT), Impact Modified
CHT Group MM239 Addition Cure 2-Part Molding Rubber

PSIKA926 / 209833

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.