MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Hexcel® HexPly® M91/34%/UD194/IM10-12K Epoxy Matrix, IM10 Carbon Fiber
Categories: Polymer; Thermoset; Epoxy; Epoxy/Carbon Fiber Composite

Material Notes:

Information provided by Hexcel Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.28 g/cc0.0462 lb/in³Resin
 1.58 g/cc0.0571 lb/in³Theoretical Calculated Laminate
 1.79 g/cc0.0647 lb/in³Fiber
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 610 MPa88500 psi(25/50/25) (gross section); ASTM D5766
 3520 MPa511000 psiASTM D3039
Tensile Modulus 176 GPa25500 ksiASTM D3039
Compressive Strength 1880 MPa273000 psiASTM D695
Compressive Modulus 0.156 GPa22.6 ksiASTM D695
Shear Strength 105 MPa15200 psiInterlaminar; EN 2563
 315 MPa45700 psiOpen Hole, (25/50/25) (gross section); ASTM D6484
 
Thermal PropertiesMetricEnglishComments
Glass Transition Temp, Tg 185 - 190 °C365 - 374 °FDMA extrapolated onset E’; EN 6032
 
Descriptive Properties
Fabric Weight194 g/m2

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHEXCB9171 / 322327

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.