MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Dow Appeel® 11D888 Ethylene Vinyl Acetate
Categories: Polymer; Thermoplastic; Ethylene Vinyl Acetate; Ethylene Vinyl Acetate Copolymer (EVA), Adhesive/Sealant Grade

Material Notes: Appeel®11D888 is a developmental modified ethylene vinyl acetate resin designed to function as a sealing layer for lidding applications. It is most often suggested to provide peelable seals over a broad temperature range to containers constructed of PP, PS & PET. Appeel® 11D888 is available in pellet form for use in conventional extrusion and coextrusion equipment designed to process polyethylene resins.

Appeel® 11D888 complies with Food and Drug Administration Regulation 21 CFR FDA Status Information 177.1350(a)(1) --Ethylene -vinyl acetate copolymers, subject to the limitations and requirements therein. This Regulation describes polymers that may be used in contact with food, subject to the finished food-contact article meeting the extractive limitations under the intended conditions of use, as shown in paragraph (b)(1) of the Regulation

This former DuPont product line is now a Dow product line.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.940 g/cc0.0340 lb/in³ASTM D792, ISO 1183
Melt Flow 32 g/10 min
@Load 2.16 kg,
Temperature 190 °C
32 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238, ISO 1133
 
Thermal PropertiesMetricEnglishComments
Melting Point 71.0 °C160 °FASTM D3418, ISO 3146
Vicat Softening Point 55.0 °C131 °FASTM D1525, ISO 306
 
Processing PropertiesMetricEnglishComments
Processing Temperature <= 235 °C<= 455 °F
Feed Temperature 140 °C284 °FExtrusion Coating
Zone 2 190 °C374 °FExtrusion Coating
Zone 3 210 °C410 °FExtrusion Coating
Zone 4 220 °C428 °FExtrusion Coating
Zone 5 220 °C428 °FExtrusion Coating
Adapter Temperature 220 °C428 °FExtrusion Coating
Die Temperature 220 °C428 °FExtrusion Coating
Melt Temperature 210 - 235 °C410 - 455 °FExtrusion Coating
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Armacell OleTex® BCJN 200 EVA/LDPE Foam
Dow Appeel® 45D747 Polyolefin
Arkema Evatane® 1003 VL 4C Ethylene Vinyl Acetate
Arkema Evatane® 1003 VL 2 Ethylene Vinyl Acetate
Arkema Evatane® 1003 VN 4 Ethylene Vinyl Acetate

PDTA4901 / 170341

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.