MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Syensqo (Solvay Specialty Polymers) Amodel® LF-1950 HS NT-9 PPA, 50% Long Glass Fiber Reinforced, Dry  (discontinued **)
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), 50% Glass Fiber Reinforced

Material Notes:

Information provided by Solvay

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.61 g/cc0.0582 lb/in³ISO 1183
Moisture Absorption 0.80 %0.80 %50% RH; ISO 62
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break  200 MPa
@Temperature 120 °C
29000 psi
@Temperature 248 °F
ISO 527
 270 MPa
@Temperature 90.0 °C
39200 psi
@Temperature 194 °F
ISO 527
 295 MPa
@Temperature 23.0 °C
42800 psi
@Temperature 73.4 °F
ISO 527
Elongation at Break 2.0 %2.0 %ISO 527
Tensile Modulus  14.8 GPa
@Temperature 120 °C
2150 ksi
@Temperature 248 °F
ISO 527
 18.0 GPa
@Temperature 90.0 °C
2610 ksi
@Temperature 194 °F
ISO 527
 18.7 GPa
@Temperature 23.0 °C
2710 ksi
@Temperature 73.4 °F
ISO 527
Flexural Strength 440 MPa63800 psiISO 178
Flexural Modulus 17.5 GPa2540 ksiISO 178
Charpy Impact Unnotched 8.50 J/cm²40.4 ft-lb/in²ISO 179
Charpy Impact, Notched 1.50 J/cm²7.14 ft-lb/in²ISO 179
 
Electrical PropertiesMetricEnglishComments
Surface Resistance 1.00e+12 ohm1.00e+12 ohmASTM D257
Dielectric Strength 35.0 kV/mm889 kV/inIEC 60243-1
Comparative Tracking Index 600 V600 VIEC 112
 
Thermal PropertiesMetricEnglishComments
CTE, linear 20.0 µm/m-°C11.1 µin/in-°FISO 7991
Thermal Conductivity 0.350 W/m-K2.43 BTU-in/hr-ft²-°FISO 22007
Deflection Temperature at 0.46 MPa (66 psi) 300 °C572 °FISO 75
Deflection Temperature at 1.8 MPa (264 psi) 285 °C545 °FISO 75
Shrinkage 0.25 %0.25 %
 
Processing PropertiesMetricEnglishComments
Zone 1 320 - 340 °C608 - 644 °F
Zone 2 320 - 335 °C608 - 635 °F
Zone 3 320 - 335 °C608 - 635 °F
Zone 4 325 - 340 °C617 - 644 °F

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSOLVAY654 / 218382

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.