MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Overview of materials for Nylon 6, Carbon Fiber Filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Carbon Fiber Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Nylon 6, Carbon Fiber Filled". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

New suppliers have been added for this product during the past 60 days.  

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.11 - 1.90 g/cc0.0401 - 0.0686 lb/in³Average value: 1.27 g/cc Grade Count:86
Filler Content 1.00 - 50.0 %1.00 - 50.0 %Average value: 29.2 % Grade Count:19
Water Absorption 0.500 - 6.80 %0.500 - 6.80 %Average value: 1.54 % Grade Count:17
Moisture Absorption at Equilibrium 0.800 - 3.32 %0.800 - 3.32 %Average value: 1.94 % Grade Count:23
Water Absorption at Saturation 3.50 - 6.50 %3.50 - 6.50 %Average value: 5.09 % Grade Count:11
Additive Loading 15.0 - 40.0 %15.0 - 40.0 %Average value: 26.3 % Grade Count:4
Maximum Moisture Content 0.0200 - 0.1500.0200 - 0.150Average value: 0.118 Grade Count:4
 0.200 - 0.200
@Temperature 120 - 120 °C
0.200 - 0.200
@Temperature 248 - 248 °F
Average value: 0.200 Grade Count:1
 0.200 - 0.200
@Time 299 - 299 sec
0.200 - 0.200
@Time 0.0830 - 0.0830 hour
Average value: 0.200 Grade Count:1
Linear Mold Shrinkage 0.000200 - 0.0110 cm/cm0.000200 - 0.0110 in/inAverage value: 0.00332 cm/cm Grade Count:48
Linear Mold Shrinkage, Transverse 0.00100 - 0.0140 cm/cm0.00100 - 0.0140 in/inAverage value: 0.00663 cm/cm Grade Count:26
Melt Flow 3.00 - 60.0 g/10 min3.00 - 60.0 g/10 minAverage value: 25.0 g/10 min Grade Count:11
Ash  10.0 - 30.0 %
@Temperature 550 - 550 °C
10.0 - 30.0 %
@Temperature 1020 - 1020 °F
Average value: 20.0 % Grade Count:2
 10.0 - 30.0 %
@Time 600 - 600 sec
10.0 - 30.0 %
@Time 0.167 - 0.167 hour
Average value: 20.0 % Grade Count:2
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 115 - 119115 - 119Average value: 116 Grade Count:8
Ball Indentation Hardness 90.0 - 320 MPa13100 - 46400 psiAverage value: 219 MPa Grade Count:7
Tensile Strength, Ultimate 1.00 - 1910 MPa145 - 277000 psiAverage value: 231 MPa Grade Count:79
Tensile Strength, Yield 138 - 221 MPa20000 - 32100 psiAverage value: 196 MPa Grade Count:8
Elongation at Break 1.00 - 20.0 %1.00 - 20.0 %Average value: 3.31 % Grade Count:80
Modulus of Elasticity 3.50 - 135 GPa508 - 19600 ksiAverage value: 19.1 GPa Grade Count:71
Flexural Yield Strength 75.0 - 1040 MPa10900 - 151000 psiAverage value: 300 MPa Grade Count:61
Flexural Modulus 3.40 - 97.9 GPa493 - 14200 ksiAverage value: 17.0 GPa Grade Count:56
Izod Impact, Notched 0.255 - 2.67 J/cm0.478 - 5.00 ft-lb/inAverage value: 1.12 J/cm Grade Count:26
Izod Impact, Unnotched 5.34 - 17.1 J/cm10.0 - 32.0 ft-lb/inAverage value: 8.87 J/cm Grade Count:14
Izod Impact, Notched (ISO) 5.00 - 30.0 kJ/m²2.38 - 14.3 ft-lb/in²Average value: 14.5 kJ/m² Grade Count:15
 11.0 - 18.0 kJ/m²
@Temperature -30.0 - -30.0 °C
5.23 - 8.57 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 14.8 kJ/m² Grade Count:6
Izod Impact, Unnotched (ISO) 45.0 - 90.0 kJ/m²21.4 - 42.8 ft-lb/in²Average value: 71.3 kJ/m² Grade Count:8
 60.0 - 93.0 kJ/m²
@Temperature -30.0 - -30.0 °C
28.6 - 44.3 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 72.2 kJ/m² Grade Count:6
Charpy Impact Unnotched 2.20 J/cm² - NB10.5 ft-lb/in² - NBAverage value: 6.02 J/cm² Grade Count:32
 4.00 - 6.51 J/cm²
@Temperature -30.0 - -20.0 °C
19.0 - 31.0 ft-lb/in²
@Temperature -22.0 - -4.00 °F
Average value: 5.01 J/cm² Grade Count:5
Charpy Impact, Notched 0.300 - 3.57 J/cm²1.43 - 17.0 ft-lb/in²Average value: 1.22 J/cm² Grade Count:42
 0.300 - 1.995 J/cm²
@Temperature -30.0 - -20.0 °C
1.43 - 9.495 ft-lb/in²
@Temperature -22.0 - -4.00 °F
Average value: 1.10 J/cm² Grade Count:5
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00500 - 1.00e+16 ohm-cm0.00500 - 1.00e+16 ohm-cmAverage value: 3.04e+14 ohm-cm Grade Count:37
Surface Resistance 0.190 - 1.00e+13 ohm0.190 - 1.00e+13 ohmAverage value: 5.03e+11 ohm Grade Count:36
 
Thermal PropertiesMetricEnglishComments
CTE, linear 3.00 - 80.0 µm/m-°C1.67 - 44.4 µin/in-°FAverage value: 23.0 µm/m-°C Grade Count:16
CTE, linear, Transverse to Flow 3.00 - 60.0 µm/m-°C1.67 - 33.3 µin/in-°FAverage value: 24.5 µm/m-°C Grade Count:4
Melting Point 200 - 315 °C392 - 599 °FAverage value: 228 °C Grade Count:41
Maximum Service Temperature, Air 100 - 260 °C212 - 500 °FAverage value: 155 °C Grade Count:10
Deflection Temperature at 0.46 MPa (66 psi) 190 - 280 °C374 - 536 °FAverage value: 217 °C Grade Count:24
Deflection Temperature at 1.8 MPa (264 psi) 170 - 282 °C338 - 540 °FAverage value: 210 °C Grade Count:49
Deflection Temperature at 8.0 MPa 100 - 240 °C212 - 464 °FAverage value: 148 °C Grade Count:6
Vicat Softening Point 165 - 255 °C329 - 491 °FAverage value: 204 °C Grade Count:17
Minimum Service Temperature, Air -60.0 - 100 °C-76.0 - 212 °FAverage value: -33.3 °C Grade Count:6
Glass Transition Temp, Tg 5.00 - 74.2 °C41.0 - 166 °FAverage value: 50.4 °C Grade Count:7
Flammability, UL94 HB - V-0HB - V-0Grade Count:37
 
Processing PropertiesMetricEnglishComments
Processing Temperature 221 - 300 °C430 - 572 °FAverage value: 262 °C Grade Count:5
Nozzle Temperature 230 - 300 °C446 - 572 °FAverage value: 265 °C Grade Count:12
Melt Temperature 220 - 340 °C428 - 644 °FAverage value: 266 °C Grade Count:54
Mold Temperature 50.0 - 135 °C122 - 275 °FAverage value: 86.7 °C Grade Count:53
Injection Velocity 30.0 - 76.2 mm/sec1.18 - 3.00 in/secAverage value: 56.1 mm/sec Grade Count:5
Drying Temperature 73.9 - 120 °C165 - 248 °FAverage value: 87.1 °C Grade Count:51
Moisture Content 0.0500 - 0.200 %0.0500 - 0.200 %Average value: 0.147 % Grade Count:21
Dew Point -17.8 °C0.000 °FAverage value: -17.8 °C Grade Count:6
Injection Pressure 30.0 - 130 MPa4350 - 18900 psiAverage value: 88.2 MPa Grade Count:15
Cushion 0.635 cm0.250 inAverage value: 0.635 cm Grade Count:3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 6, Unreinforced
Overview of materials for Nylon 6, 30% Glass Fiber Filled
Overview of materials for Nylon 6, Extruded
Overview of materials for Nylon 6, 50% Glass Fiber Filled
Overview of materials for Nylon 6, Mineral Reinforced, Impact Grade

O2441 / 77988

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.