MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Materion Brushform® 290 Beryllium Copper Alloy Strip; TM00 Temper (UNS C17200)  (discontinued **)
Categories: Metal; Nonferrous Metal; Beryllium Alloy; Copper Alloy

Material Notes: Treatment required for max strength: Mill Hardened
Stress Relaxation-% Stress Remaining after 1000 hrs @ 100°C: 97%
Stress Relaxation after 1000 hrs @ 200°C: 76%
Formability Ratio, 90° Bend, Radius/Thickness (Good Way): 0
Formability Ratio (bad Way): 0
Superficial Hardness: 30T 81-30N52

Tabulated properties apply to products after age hardening. Information supplied by Brush Wellman.

Brush Engineered Materials Inc. changed its name to Materion Corporation in March 2011.

Key Words: ASTM B-194
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.36 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B >= 98
Hardness, Rockwell C <= 31
Hardness, Vickers 225 - 309
Tensile Strength, Ultimate >= 680 MPa
Tensile Strength, Yield 510 - 670 MPa
Elongation at Break 19 - 35 %
Modulus of Elasticity 131 GPa
Fatigue Strength 280 - 310 MPa
@# of Cycles 1.00e+8
Reverse Bending (R=1)
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000660 - 0.0000101 ohm-cm17-26% IACS Conductivity
 
Thermal PropertiesOriginal ValueComments
CTE, linear 17.0 µm/m-°C
@Temperature 20.0 - 200 °C
Thermal Conductivity 105 W/m-K
Melting Point 870 - 980 °C
Solidus 870 °C
Liquidus 980 °C
 
Component Elements PropertiesOriginal ValueComments
Beryllium, Be 1.8 - 2.0 %
Co + Ni >= 0.20 %
Co + Ni + Fe <= 0.60 %
Copper, Cu 98 %as balance
Lead, Pb <= 0.020 %

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Tungsten, W
Materion Brushform® 290 Beryllium Copper Alloy Strip; TM08 Temper (UNS C17200)
Beryllium Copper, UNS C17200, TM08 Temper Strip
Materion Beryllium Copper Alloy 25 Plate & Rolled Bar; A (TB00) Temper; All Thicknesses (UNS C17200)
Materion Beryllium Copper Alloy 25 Strip; HT (TH04) Temper (UNS C17200)

NBB636 / 15256

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.