(Viewing data as-entered.
Click here
to return)
Vyncolit X6952 Novolac Phenolic
Categories:
Polymer
;
Thermoset
;
Filled/Reinforced Thermoset
;
Phenolic
;
Phenolic, Novolac, Glass Filled
Material Notes:
Glass fiber reinforced phenolic molding compound with superior mechanical properties: very high tensile and flexural strength combined with high elongation at break.
USES:
Information provided by Vyncolit, a Sumitomo Bakelite Group
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Bulk Density
0.650
g/cc
Powder Density; ISO 60
Density
1.70
g/cc
Relative Density; ISO 1183
Linear Mold Shrinkage
0.0017
cm/cm
Injection Molding; ISO 2577
Mechanical Properties
Original Value
Comments
Tensile Strength at Break
130
MPa
ISO 527
Elongation at Break
1.0 %
Tensile; ISO 527
Tensile Modulus
20.0
GPa
ISO 527
Flexural Strength
250
MPa
At Rupture; ISO 178
Flexural Modulus
17.5
GPa
ISO 178
Flexural Strain at Break
1.6 %
ISO 178
Compressive Strength
280
MPa
ISO 604
Charpy Impact Unnotched
2.10
J/cm²
ISO 179
Charpy Impact, Notched
0.500
J/cm²
ISO 179
Electrical Properties
Original Value
Comments
Volume Resistivity
4.00e+12
ohm-cm
DIN 53482
Surface Resistance
7.00e+12
ohm
IEC 93
Insulation Resistance
1.00e+11
ohm
Wet; 24 hours in water; IEC 167
1.00e+12
ohm
Dry; IEC 167
Dielectric Strength
30.0
kV/mm
IEC 243
Comparative Tracking Index
175
V
IEC 112
Thermal Properties
Original Value
Comments
CTE, linear, Parallel to Flow
20.0
µm/m-°C
@Temperature 20.0 °C
TMA
CTE, linear, Transverse to Flow
30.0
µm/m-°C
@Temperature 20.0 °C
TMA
Deflection Temperature at 1.8 MPa (264 psi)
220
°C
ISO 75 Af
Flammability, UL94
V-0
@Thickness 1.60 mm
V-0
@Thickness 4.00 mm
Shrinkage
0.020 %
Post Shrinkage; ISO 2577
Descriptive Properties
Color
Green
ISO type
PF 2 C3
Main Filler
Glass Fiber
Molding Method
Compression, transfer, injection
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
Plywood
Vyncolit X658 Novolac Phenolic
Vyncolit X680 Novolac Phenolic
Vyncolit X681 Novolac Phenolic
SGL Carbon Group Ridurid® EK 60 High Performance Graphite Filled Plastic
PVYNC012 / 72220
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.