MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Trinseo EMERGE™ ABS 5103 MED ABS, 30% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), 30% Glass Fiber Filled

Material Notes: Product Description: EMERGE™ ABS 5101 MED is a 30% glass filled ABS for use in approved medical applications. This resin exhibits a property of flow, rigidity, and dimensional stability, and has undergone biocompatibility testing based on ISO 10993 (Biological Evaluation of Medical Devices).
Main Characteristics: Rest under ISO 10993; Suitable for EtO and Radiation Sterilization
Applications: Medical Applications; Surgical Device Handles; Drug Delivery Devices; Medical Equipment

Availability: North America

Filler/Reinforcement: Glass Fiber, 30% Filler by Weight

Features: E-beam Sterilizable; Ethylene Oxide Sterilizable; Good Dimensional Stability; Good Flow; High Rigidity; Radiation Sterilizable

Uses: Medical Devices; Medical/Healthcare Applications; Structural Parts

Appearance: Opaque

Form: Pellets

Processing Method: Injection Molding

Information provided by Trinseo

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.28 g/cc0.0462 lb/in³ASTM D792
Linear Mold Shrinkage, Flow 0.015 - 0.025 cm/cm0.015 - 0.025 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.015 - 0.025 cm/cm0.015 - 0.025 in/inASTM D955
Melt Flow  3.9 g/10 min
@Load 3.80 kg,
Temperature 230 °C
3.9 g/10 min
@Load 8.38 lb,
Temperature 446 °F
ASTM D1238
 15 g/10 min
@Load 10.0 kg,
Temperature 220 °C
15 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 78.6 MPa11400 psi0.20 in/min; ASTM D638
Tensile Strength, Yield 77.2 MPa11200 psi0.20 in/min; ASTM D638
Elongation at Break 3.1 %3.1 %0.20 in/min; ASTM D638
Elongation at Yield 3.1 %3.1 %0.20 in/min; ASTM D638
Flexural Strength 108 MPa15700 psiASTM D790
Flexural Modulus 7.58 GPa1100 ksiASTM D790
Izod Impact, Notched 0.513 J/cm
@Thickness 3.20 mm
0.960 ft-lb/in
@Thickness 0.126 in
Injection Molded; ASTM D256
Izod Impact, Unnotched 2.30 J/cm
@Thickness 3.20 mm
4.30 ft-lb/in
@Thickness 0.126 in
Injection Molded; ASTM D4812
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 97.2 °C207 °FUnannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 91.7 °C197 °FUnannealed; ASTM D648
Vicat Softening Point 97.2 °C207 °FRate A (50°C/h), Loading 2 (50 N); ASTM D1525
 107 °C225 °FRate B (120°C/h), Loading 1 (10 N); ASTM D1525
 
Processing PropertiesMetricEnglishComments
Melt Temperature 220 - 260 °C428 - 500 °F
Mold Temperature 20.0 - 60.0 °C68.0 - 140 °F
Drying Temperature 80.0 °C176 °F
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTRINSE1520 / 312213

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.