MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Envalior Arnite® TV4 240 S PBT-20% Glass Reinforced (European and Asian Grade)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled

Material Notes: Arnite resins are engineered to provide specific performance in applications where DSM technology can offer value.

Arnite Molding resins:

  • Standard Unfilled and Reinforced materials
  • High modulus Flame retardant grades
  • Easy molding FR grades for connectors
  • Toughened unfilled materials for durability
  • High modulus, tight specification for critical auto components
  • Toughened reinforced resins
  • Low outgassing grades for reflector surfaces

Arnite extrusion resins: Specialized materials for specific uses

  • PET for medical applications
  • Loose buffer Optical fiber tubing
  • PET for stock shapes

Applications

  • Automotive:Connectors, sensors and E&E parts, Exterior fittings, Gear housings and motors, Brake valve bodies
  • Electrical & Electronic: Telecoms and IT connectors, Bobbins, Low voltage Power distribution, E-motor components, Lightings and Lamp fittings
  • Consumer Durables: Small Appliances
  • Other: Optical fiber tubing

Information provided by DSM.

Former DSM Engineering Plastics product line is now with Envalior.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.45 g/cc0.0524 lb/in³ISO 1183
Water Absorption 0.30 %0.30 %Sim. to ISO 62
Moisture Absorption at Equilibrium 0.15 %0.15 %Humidity Absorption; Sim. to ISO 62
Melt Flow 33.35 g/10 min
@Load 2.16 kg,
Temperature 250 °C
33.35 g/10 min
@Load 4.76 lb,
Temperature 482 °F
Calculated from Volume Flow Rate of 23 cm3/10min.; ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 110 MPa16000 psiISO 527-1/-2
Elongation at Break 2.5 %2.5 %ISO 527-1/-2
Tensile Modulus 8.50 GPa1230 ksiISO 527-1/-2
Charpy Impact Unnotched  5.00 J/cm²
@Temperature -30.0 °C
23.8 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
 5.00 J/cm²
@Temperature 23.0 °C
23.8 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  0.900 J/cm²
@Temperature -30.0 °C
4.28 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 0.900 J/cm²
@Temperature 23.0 °C
4.28 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+15 ohm-cm>= 1.00e+15 ohm-cmIEC 60093
Surface Resistance >= 1.00e+15 ohm>= 1.00e+15 ohmIEC 60093
Dielectric Constant  3.7
@Frequency 1e+6 Hz
3.7
@Frequency 1e+6 Hz
IEC 60250
 3.9
@Frequency 100 Hz
3.9
@Frequency 100 Hz
IEC 60250
Dielectric Strength 27.0 kV/mm686 kV/inIEC 60243-1
Dissipation Factor  0.0020
@Frequency 100 Hz
0.0020
@Frequency 100 Hz
IEC 60250
 0.015
@Frequency 1e+6 Hz
0.015
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 250 V250 VIEC 60112
 250 - 399 V250 - 399 VPLC 2; UL 746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 40.0 µm/m-°C
@Temperature 20.0 °C
22.2 µin/in-°F
@Temperature 68.0 °F
ISO 11359-1/-2
CTE, linear, Transverse to Flow 80.0 µm/m-°C
@Temperature 20.0 °C
44.4 µin/in-°F
@Temperature 68.0 °F
ISO 11359-1/-2
Melting Point 225 °C437 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 220 °C428 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 210 °C410 °FISO 75-1/-2
UL RTI, Electrical  140 °C
@Thickness 1.50 mm
284 °F
@Thickness 0.0591 in
UL746B
 140 °C
@Thickness 0.750 mm
284 °F
@Thickness 0.0295 in
UL746B
UL RTI, Mechanical with Impact  130 °C
@Thickness 0.750 mm
266 °F
@Thickness 0.0295 in
UL746B
 130 °C
@Thickness 1.50 mm
266 °F
@Thickness 0.0591 in
UL746B
UL RTI, Mechanical without Impact  140 °C
@Thickness 1.50 mm
284 °F
@Thickness 0.0591 in
UL746B
 140 °C
@Thickness 0.750 mm
284 °F
@Thickness 0.0295 in
UL746B
Flammability, UL94  V-2
@Thickness 0.750 mm
V-2
@Thickness 0.0295 in
IEC 60695-11-10
 V-0
@Thickness 1.60 mm
V-0
@Thickness 0.0630 in
IEC 60695-11-10
 
Descriptive Properties
Flame RetardantYes
Flame Retarding AgentYes
Injection MoldingYes
Release AgentYes
With FillersYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Envalior Pocan® DP 4035 000000 PBT, 30% Glass Fiber Reinforced
Envalior Pocan® DP 7244 000000 PBT, 30% Glass Fiber
Envalior Arnite® T06 200 /D PBT
Envalior Arnite® TM4 440 (PBT+PET)-MD20
Envalior Arnite® TV4 261 PBT-30% Glass Reinforced (European and Asian Grade)

PDSMEU358 / 31300

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.