MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Park Aerospace Nelcote® F-557 Phenolic Prepreg, Chopped Molding Compound Reinforced
Categories: Polymer; Thermoset; Phenolic

Material Notes: Nelcote® F-557 is a high purity silica filler phonic resin coated on Commercial or Aerospace grade silica fabric. F-557 is used in the manufacture of intermediate temperature ablative rocket nozzles, heat shields, and combustion chambers in highly oxidative environments.

Key Features and Benefits:

  • Provides a combination of high-strength and ablative properties for demanding applications
  • Low thermal expansion
  • Good Tack and Drape properties

Applications/Qualifications:

  • Rocket Nozzles
  • Combustion Chambers
  • Heat Shields
  • Rocket Motor Throat Sections

Information provided by Park Electrochemical Corp.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Filler Content 3.4 - 5.4 %3.4 - 5.4 %
Volatiles 2.0 - 5.0 %
@Temperature 135 °C
2.0 - 5.0 %
@Temperature 275 °F
8 min
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield  29.6 MPa
@Temperature 23.9 °C
4300 psi
@Temperature 75.0 °F
0° Direction, Dry; 325°F 2500psi; ASTM D3039b
 37.2 MPa
@Temperature 23.9 °C
5400 psi
@Temperature 75.0 °F
0° Direction, Dry; 325°F 2500psi and Post-Cure; ASTM D3039b
Tensile Modulus  15.2 GPa
@Temperature 23.9 °C
2200 ksi
@Temperature 75.0 °F
0° Direction, Dry; 325°F 2500psi and Post-Cure; ASTM D3039b
 17.2 GPa
@Temperature 23.9 °C
2500 ksi
@Temperature 75.0 °F
0° Direction, Dry; 325°F 2500psi; ASTM D3039b
Flexural Strength  58.6 MPa
@Temperature 23.9 °C
8500 psi
@Temperature 75.0 °F
Dry; 325°F 2500psi; ASTM D790
 103 MPa
@Temperature 23.9 °C
15000 psi
@Temperature 75.0 °F
Dry; 325°F 2500psi and Post-Cure; ASTM D790
Flexural Modulus 14.5 GPa
@Temperature 23.9 °C
2100 ksi
@Temperature 75.0 °F
Dry; 325°F 2500psi and Post-Cure; ASTM D790
Compressive Strength  176 MPa
@Temperature 23.9 °C
25500 psi
@Temperature 75.0 °F
Dry; 325°F 2500psi; ASTM D695
 214 MPa
@Temperature 23.9 °C
31000 psi
@Temperature 75.0 °F
Dry; 325°F 2500psi and Post-Cure; ASTM D695
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity 1.00 J/g-°C0.240 BTU/lb-°FASTM C351
Thermal Conductivity 0.389 W/m-K
@Temperature 149 °C
2.70 BTU-in/hr-ft²-°F
@Temperature 300 °F
ASTM C177
 
Processing PropertiesMetricEnglishComments
Shelf Life 6.00 Month
@Temperature 4.44 °C
6.00 Month
@Temperature 40.0 °F
 
Descriptive Properties
Nominal Prepreg Weight (oz/yd)30
Resin Flow (%)10-25325°F, 150psi
Resin Solids Content (%)30-36

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PPARK060 / 89332

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.