Physical Properties | Original Value | Comments |
---|
Density | 8.97 g/cc |
|
Mechanical Properties | Original Value | Comments |
---|
Tensile Strength, Ultimate | 860 MPa |
| 55.0 MPa @Temperature 1204 °C |
| 79.0 MPa @Temperature 1149 °C |
| 120 MPa @Temperature 1093 °C |
| 225 MPa @Temperature 982 °C |
| 400 MPa @Temperature 871 °C |
| 585 MPa @Temperature 760 °C |
| 670 MPa @Temperature 649 °C |
| 710 MPa @Temperature 538 °C |
Tensile Strength, Yield | 390 MPa @Strain 0.2 % |
| 26.0 MPa @Strain 0.2 %, Temperature 1204 °C |
| 39.0 MPa @Strain 0.2 %, Temperature 1149 °C |
| 57.0 MPa @Strain 0.2 %, Temperature 1093 °C |
| 120 MPa @Strain 0.2 %, Temperature 982 °C |
| 225 MPa @Strain 0.2 %, Temperature 871 °C |
| 270 MPa @Strain 0.2 %, Temperature 649 °C |
| 275 MPa @Strain 0.2 %, Temperature 538 °C |
| 285 MPa @Strain 0.2 %, Temperature 760 °C |
Elongation at Break | 47.7 % |
| 31.2 % @Temperature 1204 °C |
| 39.5 % @Temperature 1149 °C |
| 46.1 % @Temperature 760 °C |
| 49.6 % @Temperature 1093 °C |
| 55 % @Temperature 649 °C |
| 55.7 % @Temperature 538 °C |
| 58.9 % @Temperature 871 °C |
| 70.5 % @Temperature 982 °C |
Modulus of Elasticity | 211 GPa |
| 150 GPa @Temperature 1000 °C |
| 157 GPa @Temperature 900 °C |
| 164 GPa @Temperature 800 °C |
| 171 GPa @Temperature 700 °C |
| 177 GPa @Temperature 600 °C |
| 184 GPa @Temperature 500 °C |
| 190 GPa @Temperature 400 °C |
| 196 GPa @Temperature 300 °C |
| 202 GPa @Temperature 200 °C |
| 207 GPa @Temperature 100 °C |
Charpy Impact | 73.0 J |
|
Electrical Properties | Original Value | Comments |
---|
Electrical Resistivity | 0.000125 ohm-cm |
| 0.000125 ohm-cm @Temperature 1000 °C |
| 0.0001258 ohm-cm @Temperature 100 °C |
| 0.0001265 ohm-cm @Temperature 200 °C |
| 0.0001271 ohm-cm @Temperature 900 °C |
| 0.0001273 ohm-cm @Temperature 300 °C |
| 0.0001284 ohm-cm @Temperature 400 °C |
| 0.0001291 ohm-cm @Temperature 800 °C |
| 0.0001302 ohm-cm @Temperature 500 °C |
| 0.0001307 ohm-cm @Temperature 700 °C |
| 0.0001312 ohm-cm @Temperature 600 °C |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear | 12.7 µm/m-°C @Temperature 25.0 - 100 °C |
| 13.0 µm/m-°C @Temperature 25.0 - 200 °C |
| 13.3 µm/m-°C @Temperature 25.0 - 300 °C |
| 13.7 µm/m-°C @Temperature 25.0 - 400 °C |
| 14.0 µm/m-°C @Temperature 25.0 - 500 °C |
| 14.4 µm/m-°C @Temperature 25.0 - 600 °C |
| 14.8 µm/m-°C @Temperature 25.0 - 700 °C |
| 15.2 µm/m-°C @Temperature 25.0 - 800 °C |
| 15.7 µm/m-°C @Temperature 25.0 - 900 °C |
| 16.1 µm/m-°C @Temperature 25.0 - 1000 °C |
Specific Heat Capacity | 0.397 J/g-°C |
| 0.419 J/g-°C @Temperature 100 °C |
| 0.435 J/g-°C @Temperature 200 °C |
| 0.448 J/g-°C @Temperature 300 °C |
| 0.465 J/g-°C @Temperature 400 °C |
| 0.473 J/g-°C @Temperature 500 °C |
| 0.486 J/g-°C @Temperature 600 °C |
| 0.574 J/g-°C @Temperature 700 °C |
| 0.595 J/g-°C @Temperature 800 °C |
| 0.609 J/g-°C @Temperature 900 °C |
| 0.617 J/g-°C @Temperature 1000 °C |
Thermal Conductivity | 8.90 W/m-K |
| 10.4 W/m-K @Temperature 100 °C |
| 12.4 W/m-K @Temperature 200 °C |
| 14.4 W/m-K @Temperature 300 °C |
| 16.4 W/m-K @Temperature 400 °C |
| 18.4 W/m-K @Temperature 500 °C |
| 20.4 W/m-K @Temperature 600 °C |
| 22.4 W/m-K @Temperature 700 °C |
| 24.4 W/m-K @Temperature 800 °C |
| 26.4 W/m-K @Temperature 900 °C |
| 28.4 W/m-K @Temperature 1000 °C |
Melting Point | 1301 - 1371 °C |
Solidus | 1301 °C |
Liquidus | 1371 °C |
|
Component Elements Properties | Original Value | Comments |
---|
Aluminum, Al | 0.30 % |
Boron, B | <= 0.015 % |
Carbon, C | 0.10 % |
Chromium, Cr | 22 % |
Cobalt, Co | <= 5.0 % |
Iron, Fe | <= 3.0 % |
Lanthanum, La | 0.020 % |
Manganese, Mn | 0.50 % |
Molybdenum, Mo | 2.0 % |
Nickel, Ni | 57 % |
Silicon, Si | 0.40 % |
Tungsten, W | 14 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.