MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Sandvik 4L7 Tube and pipe, seamless
Categories: Metal; Ferrous Metal; Carbon Steel

Material Notes: Sandvik 4L7 is a carbon steel used for composite tubes.

Information provided by Sandvik

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Thermal PropertiesMetricEnglishComments
CTE, linear  12.3 µm/m-°C
@Temperature 30.0 - 100 °C
6.83 µin/in-°F
@Temperature 86.0 - 212 °F
 12.8 µm/m-°C
@Temperature 30.0 - 200 °C
7.11 µin/in-°F
@Temperature 86.0 - 392 °F
 13.5 µm/m-°C
@Temperature 30.0 - 300 °C
7.50 µin/in-°F
@Temperature 86.0 - 572 °F
 14.3 µm/m-°C
@Temperature 30.0 - 500 °C
7.94 µin/in-°F
@Temperature 86.0 - 932 °F
 14.7 µm/m-°C
@Temperature 30.0 - 400 °C
8.17 µin/in-°F
@Temperature 86.0 - 752 °F
Thermal Conductivity  42.0 W/m-K
@Temperature 500 °C
291 BTU-in/hr-ft²-°F
@Temperature 932 °F
 46.0 W/m-K
@Temperature 20.0 °C
319 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 46.0 W/m-K
@Temperature 300 °C
319 BTU-in/hr-ft²-°F
@Temperature 572 °F
 48.0 W/m-K
@Temperature 100 °C
333 BTU-in/hr-ft²-°F
@Temperature 212 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.20 %<= 0.20 %
Manganese, Mn 0.70 %0.70 %
Phosphorus, P <= 0.025 %<= 0.025 %
Silicon, Si 0.30 %0.30 %
Sulfur, S <= 0.020 %<= 0.020 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Sandvik Sanicro 63 Tube and pipe, seamless
Sandvik 6LR62 Tube and pipe, seamless
Sandvik 15Mo3 Tube and pipe, seamless
Overview of materials for Low Carbon Steel
NRI Acid Coat Flexible, Chemical Resistant, Urethane Polymer Coating

NSANDV5161 / 199725

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.