MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Celanese Hytrel® HTR8685 BK022A TPC-ET
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyester TPE

Material Notes: 44 Shore D, Lubricated, High Viscosity Polyester Elastomer with Superior Fatigue Resistance Developed for Blow Molding

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.15 g/cc0.0415 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.017 cm/cm0.017 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.016 cm/cm0.016 in/inISO 294-4, 2577
Melt Flow 0.70 g/10 min
@Load 2.16 kg,
Temperature 230 °C
0.70 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 414115s; ISO 48-4
 <= 44<= 44ISO 48-4
Tensile Stress at Strain  8.40 MPa
@Strain 10 %
1220 psi
@Strain 10 %
ISO 527-1/-2
 14.0 MPa
@Strain 50 %
2030 psi
@Strain 50 %
ISO 527-1/-2
 19.0 MPa
@Strain 100 %
2760 psi
@Strain 100 %
ISO 527-1/-2
Flexural Modulus 0.100 GPa14.5 ksiISO 178
Charpy Impact, Notched  12.0 J/cm²
@Temperature -40.0 °C
57.1 ft-lb/in²
@Temperature -40.0 °F
ISO 179/1eA
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eA
Tear Strength 109 kN/m622 plinormal; ISO 34-1
 112 kN/m639 pliparallel; ISO 34-1
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 210 µm/m-°C117 µin/in-°FISO 11359-1/-2
CTE, linear, Transverse to Flow 200 µm/m-°C111 µin/in-°FISO 11359-1/-2
Melting Point 206 °C403 °F10°C/min; ISO 11357-1/-3
Glass Transition Temp, Tg -30.0 °C-22.0 °F10°C/min; ISO 11357-1/-2
Flame Spread <= 80.0 mm/min
@Thickness 1.00 mm
<= 3.15 in/min
@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
 
Processing PropertiesMetricEnglishComments
Melt Temperature 240 °C464 °FOptimum, Injection
 230 - 250 °C446 - 482 °FRange, Injection
Mold Temperature 45.0 °C113 °FOptimum, Injection
 40.0 - 50.0 °C104 - 122 °FInjection
Drying Temperature 100 °C212 °FInjection
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hourBlow Molding, Dehumidified Dryer
 3.00 - 4.00 hour3.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.020 %<= 0.020 %Blow Molding
 <= 0.080 %<= 0.080 %Injection
 
Descriptive Properties
Drying RecommendedyesInjection
FMVSS ClassBISO 3795 (FMVSS 302)
Part Marking Code>TPC-ET<ISO 11469
PolymerTPC
Regional AvailabilityAsia Pacific
 Europe
 Global
 Near East/Africa
 North America
 South and Central America
Resin IdentificationTPC-ETISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Hytrel® HTR8223 BK320 TPC-ET
DuPont Mobility and Materials Hytrel® HTR8139BK TPC-ET
Celanese Hytrel® HTR8341C BK320 TPC-ET
DuPont Mobility and Materials Hytrel® HTR8341G BK320 TPC-ET
Celanese Hytrel® 8238 TPC-ET

PDSX5217 / 197857

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.