MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Westlake Plastics

(Viewing data as-entered. Click here to return)
Westlake Plastics Pomalux® Acetal Copolymer
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM); Acetal Copolymer, Unreinforced

Material Notes: Pomalux® POMC Polyoxymethylene is a high-performance acetal copolymer. Pomalux® POMC is a 100% recyclable, semi-crystalline engineering thermoplastic most commonly used for a wide range of engineering applications. Pomalux® POMC has excellent mechanical, electrical, and wear properties. It is engineered to provide outstanding dimensional stability, even when machining parts with complex geometries. Pomalux® POMC is an excellent choice for many bearing and wear applications since it has low coefficient of friction and wears well in both wet and dry environments. It is widely used for assembly jigs and fixtures because of its inherent dimensional stability and excellent wear properties. These include automotive, electrical & electronics, industrial, and drug delivery applications, gears, bearings, snap fittings, and many other engineering components. Pomalux® POMC is often specified for electrical applications when low moisture absorption and high dielectric strength are required. Both natural (white) and black Pomalux® POMC are FDA compliant for use in food processing machinery. Westlake Plastics manufactures all Acetal extruded & compression molded sheets, plates, and rods in accordance with ASTM D6100. This specification covers requirement and test methods for the material, dimensions, workmanship and the properties of extruded and compression molded sheets, plates and rods.

Industry: Chemical Process; Engineering; Semiconductor and ESD

Colors Available: Black, Natural

Attributes: Chemical Resistance; Dielectric Properties; Wear Resistance; Food Contact

Shapes: Extruded Slab; Compression Sheet; Extruded Sheet; Extruded Rod

Information provided by Westlake Plastics Co.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.41 g/ccASTM D792
Water Absorption 0.20 %
@Time 86400 sec
ASTM D570
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 78ASTM D785
Tensile Strength, Yield 8800 psi
@Temperature 22.8 °C
ASTM D638
 13700 psi
@Temperature -40.0 °C
ASTM D638
Elongation at Break 30 %
@Temperature -40.0 °C
ASTM D638
 75 %
@Temperature 22.8 °C
ASTM D638
Tensile Modulus 357000 psiASTM D638
Flexural Modulus 375000 psiASTM D790
Compressive Strength 16000 psi10% deflection; ASTM D695
Izod Impact, Notched 1.20 ft-lb/in
@Temperature -40.0 °C
ASTM D256
 1.50 ft-lb/in
@Temperature 22.8 °C
ASTM D256
 
Thermal PropertiesOriginal ValueComments
CTE, linear 120 µin/in-°FASTM D696
Deflection Temperature at 1.8 MPa (264 psi) 230 °FASTM D648
Flammability, UL94 HB
 
Descriptive Properties
ColorNatural (white) FDA

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Westlake Plastics Pomalux® Acetal Copolymer For Medical Applications
BASF Ultraform® H 2320 006 Q600 POM
BASF Ultraform® W 2320 003 UNC Q600 POM
BASF Ultraform® W 2320 003 BK120 Q600 POM
Ensinger Tecaform™ SAN Polyacetal (POM)

PWEST006 / 72710

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.