MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
DuPont Mobility and Materials Zytel® RS LC4601 NC010 PA-IP  (discontinued **)
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Nylon (Polyamide PA)

Material Notes: Plasticized, Toughened, Renewably Sourced, Polyamide Developed for Extrusion

While this product line has been acquired by Celanese, this specific grade had been disconued while still a DuPont product so it is listed here as a discontinued DuPont product.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.04 g/ccDAM; ISO 1183
Moisture Absorption 1.00 %
@Thickness 2.00 mm
DAM; Sim. to ISO 62
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 33.3 MPaDAM; ISO 527-1/-2
Tensile Stress at Strain 25.0 MPa
@Strain 50 %
50% RH; ISO 527-1/-2
Elongation at Break >= 50 %50% RH; ISO 527-1/-2
 380 %50mm/min; 50% RH; ISO 527-1/-2
Elongation at Yield 13 %DAM; ISO 527-1/-2
Tensile Modulus 750 MPaDAM; ISO 527-1/-2
Flexural Modulus 700 MPaDAM; ISO 178
Poissons Ratio 0.46DAM; ISO 527-1/-2
Izod Impact, Unnotched (ISO) 15.0 kJ/m²
@Temperature -40.0 °C
DAM; ISO 180/1A
 75.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
Charpy Impact Unnotched NB
@Temperature 23.0 °C
DAM; ISO 179/1eU
 NB
@Temperature -30.0 °C
DAM; ISO 179/1eU
Charpy Impact, Notched 15.0 kJ/m²
@Temperature -40.0 °C
DAM; ISO 179/1eA
 95.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Melting Point 214 °C10°C/min; DAM; ISO 11357-1/-3
Glass Transition Temp, Tg 30.0 °C10°C/min; 50% RH; ISO 11357-1/-2
 50.0 °C10°C/min; DAM; ISO 11357-1/-2
Flame Spread <= 80.0 mm/min
@Thickness 1.00 mm
ISO 3795 (FMVSS 302)
 
Processing PropertiesOriginal ValueComments
Melt Temperature 235 °CExtrusion Optimum
 230 - 245 °CExtrusion
Drying Temperature 75.0 °CExtrusion
 80.0 °CExtrusion
Dry Time 3.00 - 4.00 hourDehumidified Dryer; Extrusion
Moisture Content 0.060 %Extrusion
 
Descriptive Properties
AdditivesPlasticizer
Delivery formPellets
FMVSS ClassBISO 3795 (FMVSS 302)
Part Marking Code>PA-IP<ISO 11469
ProcessingInjection Molding
 Other Extrusion
 Profile Extrusion
Resin IdentificationPA-IPISO 1043
Special characteristicsHeat stabilized or stable to heat

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PZDSX5501 / 198141

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.