MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Teknor Apex Sarlink® TPE OM-1354 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Sarlink OM series are high performance specialty thermoplastic elastomers designed for automotive applications requiring excellent bondability to engineered resin substrates. Sarlink OM-1354 is a medium hardness, low density, opaque grade that exhibits excellent adhesion to nylon (polyamide).

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Bondability; Chemical Resistant; Good Adhesion; Good Colorability; Good Processability; Low Density; Low Specific Gravity; Medium Hardness

Uses: Automotive Applications; Automotive Interior Trim; Bonding; Flexible Grips; Handles; Knobs; Overmolding; Rubber Replacement; Soft Touch Applications

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding; Multi Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.920 g/cc0.0332 lb/in³ASTM D792
Melt Flow 33 g/10 min
@Load 2.16 kg,
Temperature 190 °C
33 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 5656ASTM D2240
 54
@Time 5.00 sec
54
@Time 0.00139 hour
ASTM D2240
Tensile Strength at Break 3.38 MPa490 psiAcross Flow; ASTM D412
 4.07 MPa590 psiFlow; ASTM D412
Elongation at Break 280 %280 %Across Flow; ASTM D412
 440 %440 %Flow; ASTM D412
Tear Strength 19.3 kN/m110 pliFlow; ASTM D624
 21.0 kN/m120 pliAcross Flow; ASTM D624
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 204 - 232 °C400 - 450 °F
Middle Barrel Temperature 210 - 232 °C410 - 450 °F
Front Barrel Temperature 216 - 238 °C420 - 460 °F
Nozzle Temperature 221 - 243 °C430 - 470 °F
Melt Temperature 221 - 243 °C430 - 470 °F
Mold Temperature 23.9 - 60.0 °C75.0 - 140 °F
Drying Temperature 65.6 °C150 °F
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hour
Injection Pressure 1.38 - 6.89 MPa200 - 1000 psi
Back Pressure 0.172 - 0.862 MPa25.0 - 125 psi
Cushion 0.381 - 2.54 cm0.150 - 1.00 in
Screw Speed 50 - 120 rpm50 - 120 rpm
 
Descriptive Properties
AppearanceColors Available
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ1120 / 237611

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.