MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Evonik Paraglas Soundstop® Transparent Sheet  (discontinued **)
Categories: Polymer; Thermoplastic; Acrylic (PMMA); Acrylic, Optical Sheet

Material Notes: Paraglas Soundstop is a standard clear transparent sheet

Information provided by Cyro Industries

Information Provided by Evonik CYRO. The former Evonik Methacrylates business has been sold to Röhm GmbH, although this trade name was disontinued prior to the sale.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.19 g/cc0.0430 lb/in³ASTM D792
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 69.0 MPa10000 psiASTM D638
Elongation at Break 4.5 %4.5 %ASTM D638
Tensile Modulus 2.80 GPa406 ksiASTM D638
Flexural Strength 117 MPa17000 psiASTM D790
Flexural Modulus 3.30 GPa479 ksiASTM D790
Compressive Strength 117 MPa17000 psiASTM D695
Charpy Impact Unnotched 1.365 J/cm²6.496 ft-lb/in²Weathered 5 years; ASTM D4812
 1.365 J/cm²6.496 ft-lb/in²At -5°F; ASTM D4812
 1.365 J/cm²6.496 ft-lb/in²ASTM D4812
Sound Insulation  32 dB
@Thickness 15.0 mm
32 dB
@Thickness 0.591 in
ASTM E 90
 34 dB
@Thickness 20.0 mm
34 dB
@Thickness 0.787 in
ASTM E 90
 36 dB
@Thickness 25.0 mm
36 dB
@Thickness 0.984 in
ASTM E 90
 
Thermal PropertiesMetricEnglishComments
CTE, linear 72.0 µm/m-°C
@Temperature 20.0 °C
40.0 µin/in-°F
@Temperature 68.0 °F
ASTM D696
Maximum Service Temperature, Air >= 71.1 °C>= 160 °F
Deflection Temperature at 1.8 MPa (264 psi) 90.6 °C195 °FASTM D648
Vicat Softening Point 105 °C221 °FASTM D1525
Flame Spread 15 mm/min
@Thickness 15.0 mm
0.60 in/min
@Thickness 0.591 in
ASTM D635
Smoke Density 20
@Thickness 15.0 mm
20
@Thickness 0.591 in
percent; ASTM D2843
Ignition Temperature 454 °C850 °FSelf Ignition; ASTM D1929
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.491.49ASTM D542
Haze 1.0 %1.0 %ASTM D1003
 1.5 %1.5 %Weathered 5 years AZ; ASTM D1003
Yellow Index <= 1.0 %<= 1.0 %ASTM E 313
 1.5 %1.5 %Weathered 5 years AZ; ASTM E 313
Transmission, Visible 92 %92 %Weathered 5 years AZ
 92 %92 %ASTM D1003
 
Descriptive Properties
Resistance to BrushfireClass215mm, EN1794-2
Resistance to stone projectilesPass15mm, EN1794-1

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PCYRO05 / 29182

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.