MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

SABIC ULTEM™ Resin 4002 Polyetherimide (PEI)
Categories: Polymer; Thermoplastic; Polyetherimide (PEI)

Material Notes: PTFE filled, standard flow Polyetherimide (Tg 217C). ECO Conforming, UL 94 V0 and 5VA listing in recognized colors.

Features: High Stiffness,Hydrolytic Stability,Chemical Resistance,Low Smoke and Toxicity,Good Mechanicals in Broad Temperature Range,Low Creep Sensitivity,Low Shrinkage,Good metal adhesion,Amorphous,High Strength,High Heat Resistance,Good dimensional stability,Flame Retardant,Wear resistant

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.33 g/cc1.33 g/ccASTM D792
Density 1.33 g/cc0.0480 lb/in³ISO 1183
Moisture Absorption 0.0200 %0.0200 %Injection Molding
 0.600 %0.600 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 1.1 %1.1 %ISO 62-1
Viscosity 13 cP
@Load 5.00 kg,
Temperature 360 °C
13 cP
@Load 11.0 lb,
Temperature 680 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0060 - 0.0080 cm/cm0.0060 - 0.0080 in/inSABIC method
 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
0.0050 - 0.0070 in/in
@Thickness 0.126 in
SABIC method
Linear Mold Shrinkage, Transverse 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
0.0050 - 0.0070 in/in
@Thickness 0.126 in
SABIC method
Melt Flow 9.5 g/10 min
@Load 6.60 kg,
Temperature 337 °C
9.5 g/10 min
@Load 14.6 lb,
Temperature 639 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 80.0 MPa11600 psi50 mm/min; ISO 527
 85.0 MPa12300 psi5 mm/min; ASTM D638
Tensile Strength, Yield 100 MPa14500 psi50 mm/min; ISO 527
 105 MPa15200 psi5 mm/min; ASTM D638
Elongation at Break 25 %25 %50 mm/min; ISO 527
 40 %40 %5 mm/min; ASTM D638
Elongation at Yield 5.0 %5.0 %5 mm/min; ASTM D638
 6.0 %6.0 %50 mm/min; ISO 527
Tensile Modulus 3.30 GPa479 ksi1 mm/min; ISO 527
 3.46 GPa502 ksi5 mm/min; ASTM D638
Flexural Strength 130 MPa18900 psiyield, 2 mm/min; ISO 178
 155 MPa22500 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 3.10 GPa450 ksi2 mm/min; ISO 178
 3.55 GPa515 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 117 J86.3 ft-lbASTM D256
 120 J
@Temperature -30.0 °C
88.5 ft-lb
@Temperature -22.0 °F
ASTM D256
Izod Impact, Notched (ISO) 10.0 kJ/m²4.76 ft-lb/in²80*10*4; ISO 180/1A
 8.00 kJ/m²
@Temperature -30.0 °C
3.81 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
Charpy Impact, Notched 1.10 J/cm²5.23 ft-lb/in²Edgew 80*10*4 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 380 J280 ft-lbASTM D3763
 
Electrical PropertiesMetricEnglishComments
Arc Resistance 60 - 120 sec60 - 120 secASTM D495
Comparative Tracking Index 100 - 175 V100 - 175 VUL 746A
Hot Wire Ignition, HWI  30 - 60 sec
@Thickness >=1.60 mm
30 - 60 sec
@Thickness >=0.0630 in
UL 746A
 60 - 120 sec
@Thickness >=3.00 mm
60 - 120 sec
@Thickness >=0.118 in
UL 746A
High Amp Arc Ignition, HAI  0.00 - 15 arcs
@Thickness >=1.60 mm
0.00 - 15 arcs
@Thickness >=0.0630 in
UL 746A
 15 - 30 arcs
@Thickness >=3.00 mm
15 - 30 arcs
@Thickness >=0.118 in
UL 746A
High Voltage Arc-Tracking Rate, HVTR 25.4 - 80.0 mm/min1.00 - 3.15 in/minUL 746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  39.0 µm/m-°C
@Temperature -40.0 - 150 °C
21.7 µin/in-°F
@Temperature -40.0 - 302 °F
ASTM E831
 39.0 µm/m-°C
@Temperature 23.0 - 150 °C
21.7 µin/in-°F
@Temperature 73.4 - 302 °F
ISO 11359-2
CTE, linear, Transverse to Flow  40.0 µm/m-°C
@Temperature -40.0 - 150 °C
22.2 µin/in-°F
@Temperature -40.0 - 302 °F
ASTM E831
 40.0 µm/m-°C
@Temperature 23.0 - 150 °C
22.2 µin/in-°F
@Temperature 73.4 - 302 °F
ISO 11359-2
Hot Ball Pressure Test 125 °C257 °FPASS; IEC 60695-10-2
Deflection Temperature at 1.8 MPa (264 psi) 190 °C374 °FEdgew 120*10*4 sp=100mm; ISO 75/Ae
 197 °C
@Thickness 3.20 mm
387 °F
@Thickness 0.126 in
unannealed; ASTM D648
 200 °C
@Thickness 6.40 mm
392 °F
@Thickness 0.252 in
unannealed; ASTM D648
Vicat Softening Point 210 °C410 °FRate B/120; ISO 306
 215 °C419 °FRate B/50; ISO 306
 219 °C426 °FRate B/50; ASTM D1525
UL RTI, Electrical 170 °C338 °FUL 746B
UL RTI, Mechanical with Impact 170 °C338 °FUL 746B
UL RTI, Mechanical without Impact 170 °C338 °FUL 746B
Flammability, UL94  V-0
@Thickness >=0.380 mm
V-0
@Thickness >=0.0150 in
UL 94
 5VA
@Thickness >=1.90 mm
5VA
@Thickness >=0.0748 in
UL 94
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 350 - 370 °C662 - 698 °F
Zone 2 345 - 365 °C653 - 689 °F
Zone 3 350 - 370 °C662 - 698 °F
Melt Temperature 350 - 370 °C662 - 698 °FInjection Molding
Mold Temperature 135 - 165 °C275 - 329 °F
Drying Temperature 135 °C275 °FInjection Molding
Dry Time 4.00 - 6.00 hour4.00 - 6.00 hourInjection Molding
 10.0 hour10.0 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 40 - 60 %40 - 60 %
Vent Depth 0.00250 - 0.00760 cm0.000984 - 0.00299 in
Screw Speed 40 - 70 rpm40 - 70 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH82550 / 290497

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.