MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Copper Alloy, UNS C42200, OS035 Temper, Flat Products
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Temper: Nominal Grain Size 0.035 mm

Fabrication Properties: Excellent Suitability – Soldering, Gas Shielded Arc Welding, Capacity for Being Cold Worked; Good Suitability – Spot Weld, Butt Weld, Capacity for Being Hot Formed; Fair Suitability – Brazing, Seam Weld

Common Fabrication Processes: Blanking; Drawing; Forming; Piercing and Punching

Typical Uses: Connectors; Electrical Connectors; Fuse Clips; Terminals; Spring Washers; Bushings; Contact Springs; Sash Chain

Applicable Specifications: Bar – ASTM B591; Plate – ASTM B591; Sheet - ASTM B591; Strip – ASTM B888/B88M, ASTM B591

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.80 g/cc0.318 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell F 6565
Hardness, Rockwell 30T 2727
Tensile Strength 296 MPa43000 psi
Tensile Strength, Yield 96.5 MPa14000 psi0.2% Offset
 103 MPa15000 psi0.5% Ext
Elongation at Break 46 %46 %
Tensile Modulus 124 GPa18000 ksi
Machinability 30 %30 %
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000550 ohm-cm0.00000550 ohm-cm31% IACS
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity 0.377 J/g-°C0.0900 BTU/lb-°F
Thermal Conductivity 10.8 W/m-K75.0 BTU-in/hr-ft²-°F
Melting Point 1020 - 1041 °C1870 - 1905 °F
Solidus 1020 °C1870 °F
Liquidus 1041 °C1905 °F
Annealing Point 499 - 677 °C930 - 1250 °F
 
Processing PropertiesMetricEnglishComments
Hot-Working Temperature 829.4 - 890.6 °C1525 - 1635 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 86 - 89 %86 - 89 %
Iron, Fe <= 0.050 %<= 0.050 %
Lead, Pb <= 0.050 %<= 0.050 %
Phosphorus, P <= 0.35 %<= 0.35 %
Tin, Sn 0.80 - 1.4 %0.80 - 1.4 %
Zinc, Zn 9.2 - 13.2 %9.2 - 13.2 %As Balance
 
Descriptive Properties
US EPA Registered AntimicrobialYes

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

MC42200x9 / 291921

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.