MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Evonik VESTAMID® X7293 BK 9.7507 Nylon 12, Conditioned
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12)

Material Notes: VESTAMID® X7293 BK 9.7507 is a plasticized polyamide 12 compound with heat and light stabilizer for the extrusion of flexible tubing and hose, especially for automotive applications according to DIN 73378, (PA 12-HIPHL, Type 1), ISO/DIN 7628-1 (PA 12-HIPEHL, Type 1) and SAE J844. VESTAMID® X7293 BK 9.7507 is distinguished by an easy processing as well as by a high impact strength at low temperatures. Properties of compounds based on Polyamide 12 vary little with changing humidity due to low moisture absorption. Parts made of this semicrystalline material are characterized by exceptional impact strength, low coefficient of friction and good chemical resistance. VESTAMID® X7293 BK 9.7507 is supplied as cylindrical granules, ready for use, in moisture-proof bags. Inside the original and undamaged packaging, the product has a shelf life of at least 2 years when stored in dry rooms at temperatures not exceeding 30°C.
Industrial Sector: Automotive and Mobility, Sustainable, Industry and Engineering
Sustainability Sustainable electricity
Processing: Injection molding, Extrusion
Delivery form: Pellets, Granules
Resistance to: Heat (thermal stability), UV / light / weathering, Oil / fuels
Electrical: Insulating
Conformity: Automotive
Additives: Lubricant, Unfilled
Applications: Tube and hose
Processing: Profile extrusion, Pipe/Tube extrusion
Special Characteristics: High impact strength, Light-stabilized, High heat resistant
Features: Low coefficient of friction
Color: Black
Additives: Plasticizer, Impact resistant, Light stabilizer, Heat stabilizer
Chemical Resistance: General chemical resistance

Information provided by Evonik.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 40.0 MPa5800 psiISO 527
Tensile Strength 24.0 MPa3480 psiISO 527
Tensile Stress  24.0 MPa
@Strain 50.0 %
3480 psi
@Strain 50.0 %
ISO 527
 24.0 MPa
@Strain 50.0 %
3480 psi
@Strain 50.0 %
ISO 527
Tensile Strength, Yield 24.0 MPa3480 psiISO 527
Elongation at Break 250 %250 %Nominal; ISO 527
Elongation at Yield 32.0 %32.0 %ISO 527
Tensile Modulus 0.400 GPa58.0 ksiISO 527
Flexural Strength 13.0 MPa1890 psiat conv. Deflection; ISO 178
 21.0 MPa3050 psiISO 178
Flexural Modulus 0.390 GPa56.6 ksiISO 178
Flexural Strain at Break 9.00 %9.00 %at flexural strength; ISO 178
Charpy Impact Unnotched  NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eU
 NB
@Temperature 0.000 °C
NB
@Temperature 32.0 °F
ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
Charpy Impact, Notched  0.600 J/cm²
@Temperature -30.0 °C
2.86 ft-lb/in²
@Temperature -22.0 °F
Type of failure: C; ISO 179/1eA
 12.5 J/cm²
@Temperature 23.0 °C
59.5 ft-lb/in²
@Temperature 73.4 °F
Type of failure: P; ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 2.70e+9 ohm-cm2.70e+9 ohm-cmIEC 62631-3-1
Surface Resistance 1.90e+13 ohm1.90e+13 ohmcircular electrodes; IEC 62631-3-2
Dielectric Constant  3.70
@Frequency 1.00e+6 Hz
3.70
@Frequency 1.00e+6 Hz
IEC 62631-2-1
 12.0
@Frequency 100 Hz
12.0
@Frequency 100 Hz
IEC 62631-2-1
 13.0
@Frequency 50.0 Hz
13.0
@Frequency 50.0 Hz
IEC 62631-2-1
Dielectric Strength 37.0 kV/mm
@Thickness 1.00 mm
940 kV/in
@Thickness 0.0394 in
AC, S20/S20, t.; IEC 60243-1
Dissipation Factor  0.145
@Frequency 1.00e+6 Hz
0.145
@Frequency 1.00e+6 Hz
IEC 62631-2-1
 0.147
@Frequency 100 Hz
0.147
@Frequency 100 Hz
IEC 62631-2-1
 0.155
@Frequency 50.0 Hz
0.155
@Frequency 50.0 Hz
IEC 62631-2-1
Comparative Tracking Index 600 V600 Vtest solution A, 50 drops value; IEC 60112
 
Descriptive Properties
ColorBlack
Flexural stress at breakNMPa, ISO 178
 N%, ISO 178

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PEVONIK7942 / 325074

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.