MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Lubrizol Estane® S385AH Thermoplastic Polyurethane  (discontinued **)
Categories: Polymer; Thermoplastic; Polyurethane, TP; Thermoplastic Polyurethane (TPUR), Polyester Grade

Material Notes: Type: Estane® S385AH is a Shore 87A, polyester based thermoplastic polyurethane (TPU) with excellent transparency and Hydrolytic Stabilizer. FDA approved (21 CFR 177.2600, 177.1680).

Uses: Injection Molding, Extrusion.

Availability: Americas, Europe, Middle East, Africa and India

Information Provided by The Lubrizol Corporation

Key Words: TPU
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.20 g/ccASTM D792
Linear Mold Shrinkage 0.026 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 87ASTM D2240
Tensile Strength, Ultimate 450 kg(f)/cm²ASTM D412
Tensile Strength, Yield 70.0 kg(f)/cm²at 100% elongation; ASTM D412
 180 kg(f)/cm²at 300% elongation; ASTM D412
Elongation at Break 700 %ASTM D412
Tear Strength 95.0 kg(f)/cmDie C; ASTM D624
Abrasion 35mm3 loss; ISO 4649
Compression Set 15 %
@Temperature 23.0 °C,
Time 79200 sec
ASTM D395
 45 %
@Temperature 70.0 °C,
Time 79200 sec
ASTM D395
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 62.0 °CASTM D1525
 
Processing PropertiesOriginal ValueComments
Feed Temperature 180 - 195 °C
Nozzle Temperature 190 - 205 °C
Mold Temperature 10.0 - 40.0 °C
Drying Temperature 70.0 - 80.0 °C
Dry Time 4.00 - 5.00 hour
Injection Pressure 1700 - 2300 psi
Hold Pressure 1200 - 1800 psi
Back Pressure 30.0 - 80.0 psi
Cycle Time - Injection 25 - 35 sec
Screw Speed 180 - 220 rpm
 
Compliance PropertiesOriginal ValueComments
FDA Yes
 
Descriptive Properties
Injection Time (s)12-18
Metering Zone185-200°C

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Lubrizol Estane® CS195A Thermoplastic Polyurethane
Lubrizol Estane® L194A Thermoplastic Polyurethane
Lubrizol Estane® 58252 Thermoplastic Polyurethane
Lubrizol ESTANE® 5799 Ester Based Thermoplastic Polyurethane
Lubrizol ESTANE® 5735 Ester Based Thermoplastic Polyurethane

PNOVEON528 / 121419

Polyurethane

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.