MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
High-leaded brass, UNS C34200
Categories: Metal; Nonferrous Metal; Copper Alloy; Brass

Material Notes: Fair to excellent corrosion resistance. Combines excellent machinability with moderate cold workability.

Applications: clock plates and nuts, clock and watch backs, gears, wheels and channel plate.

Available as flat products and rod.

Key Words: CZ119, ISO CuZn35Pb2, CEN CW601N, free-cutting brass
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.50 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 338 - 586 MPa
Tensile Strength, Yield 117 - 427 MPaDepending on temper
Elongation at Break 52 %in 127 mm.
Modulus of Elasticity 105 GPa
Poissons Ratio 0.35Calculated
Machinability 90 %UNS C36000 (free-cutting brass) = 100%
Shear Modulus 39.0 GPa
 
Thermal PropertiesOriginal ValueComments
CTE, linear 20.3 µm/m-°C
@Temperature 20.0 - 300 °C
Thermal Conductivity 115 W/m-K
@Temperature 20.0 °C
Melting Point 885 - 910 °C
Solidus 885 °C
Liquidus 910 °C
 
Component Elements PropertiesOriginal ValueComments
Copper, Cu 62.5 - 66.5 %
Iron, Fe <= 0.10 %
Lead, Pb 1.5 - 2.5 %
Other, total <= 0.50 %
Zinc, Zn 33.5 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
High-leaded brass, 62%, UNS C35300
Forging Brass, UNS C37700
Low-leaded brass, UNS C33500
Medium-leaded brass, UNS C35000, H03 Temper flat products
Free-Cutting Brass, UNS C36000

MC34200b1 / 11200

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.