MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Huntsman IROGRAN® PS455-203 TPU-Polyester
Categories: Polymer; Thermoplastic; Polyurethane, TP; Thermoplastic Polyurethane (TPUR), Polyester Grade

Material Notes: Polyester-based grades with a broad processing window ideally suited for cast, flat die and flown film lines.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.19 g/cc0.0430 lb/in³ASTM D792
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7878ASTM D2240
Hardness, Shore D 3030ASTM D2240
Tensile Strength at Break 21.5 MPa3120 psiASTM D412
Elongation at Break 570 %570 %ASTM D412
50% Modulus 1.10 MPa
@Strain 50 %
1.10 MPa
@Strain 50 %
ASTM D412
100% Modulus 1.52 MPa
@Strain 100 %
220 psi
@Strain 100 %
ASTM D412
300% Modulus 6.14 MPa
@Strain 300 %
890 psi
@Strain 300 %
ASTM D412
Rebound 50 %50 %Bayshore; ASTM D2632
Tear Strength 61.4 kN/m350 pliASTM D624
Taber Abrasion, mg/1000 Cycles 3636ASTM D3389
Abrasion 134134mm3; DIN 53516
Compression Set  35 %
@Temperature 22.8 °C,
Time 79200 sec
35 %
@Temperature 73.0 °F,
Time 22.0 hour
ASTM D395
 91 %
@Temperature 70.0 °C,
Time 79200 sec
91 %
@Temperature 158 °F,
Time 22.0 hour
ASTM D395
 
Thermal PropertiesMetricEnglishComments
Melting Point 119 - 139 °C246 - 282 °FTMA Melt Range
Vicat Softening Point 55.0 °C131 °FASTM D1525
Glass Transition Temp, Tg -39.0 °C-38.2 °FMidpoint; ASTM E 1269

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Huntsman IROGRAN® A 92 E 4738 Polyester-Based TPU-Injection Extrusion Grade
Huntsman IROGRAN® PS 370-202 TPU-Polyester
Huntsman IROGRAN® A 92 K 5031 TPU-High Temperature Performance
Huntsman IROGRAN® A 92 K 4107 TPU-High Temperature Performance
Huntsman IROGRAN® PS 440-200 TPU-Polyester

PHUQ111 / 159484

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.