MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Domo TECHNYL® B 218 V30 Black 21 N PA66, 30% glass fiber, Conditioned
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled

Material Notes: Description: Copolyamide PA66/6, reinforced with 30% of glass fiber, heat stabilized, for injection molding.

Available in: Asia Pacific and Europe

Product Applications: TECHNYL® B 218 V30 is used in all sectors of industry, offering an excellent combination between thermal and mechanical properties. This grade is commonly used in the automotive industry; especially for the production of unpainted external parts due to its excellent surface finish, such as: door mirror housing, door handles. This product is available in grey and black.

DOMO Chemicals has acquired Solvay’s Performance Polyamides Business in Europe.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.37 g/ccISO 1183/A
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 115 MPaISO 527 Type 1A
Tensile Modulus 6500 MPaISO 527 Type 1A
Flexural Modulus 4700 MPaISO 178
Izod Impact, Notched (ISO) 19.0 kJ/m²ISO 180/1eA
Charpy Impact Unnotched 92.0 kJ/m²ISO 179/1eU
Charpy Impact, Notched 16.0 kJ/m²ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.50e+12 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohmIEC 60093
Dielectric Constant 4.0IEC 60250
Dielectric Strength 29.0 kV/mmIEC 60243
Dissipation Factor 0.11IEC 60250
 
Processing PropertiesOriginal ValueComments
Moisture Content <= 0.20 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Domo TECHNYL® B 218 V30 Black 21 N PA66, 30% glass fiber, DRY
Domo TECHNYL® A 218 V30 Black 21 NS PA 66 30% Glass Reinforced, Dry
Domo TECHNYL® A 218 V30 Black 21 NS PA 66 30% Glass Reinforced, Conditioned
Domo TECHNYL® A 218 V30 PA66, 30% glass fiber, DRY
Domo TECHNYL® C 218 V 30 PA6, 30% glass fiber, DRY

PRHOD736 / 137967

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.