MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Schmolz + Bickenbach Formadur® 2083 Superclean Plastic Mold Steel
Categories: Metal; Ferrous Metal; Martensitic; Tool Steel; Mold Steel

Material Notes: Description: Formadur 2083 Superclean is an electro slag remelted (ESR) martensitic stainless steel developed for corrosion resistant applications and Supplied in the annealed condition

Characteristics: Good corrosion resistance; Good polishability; and High Hardness

Applications: Molds for processing corrosive plastics and Extrusion dies for processing corrosive plastics

Stress Relieving (Heat Treatment): 1200°F; Cooling: Furnace hold time 2 hours slowly cool in furnace to 920°F and them air cool; Hardness: <230 HB

Hardening (Heat Treatment): 1830°F- 1920°F Hold at temperature for 30 minutes; Cooling: Quench to 300°F then cool to below 150°F; Hardness: <56 HRC Quenched

Information provided by Schmolz + Bickenbach

Key Words: AISI 420 Modified
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.282 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell C 46
@Treatment Temp. 650.0 °C
 49
@Treatment Temp. 600.0 °C
 54
@Treatment Temp. 300 °C
 54
@Treatment Temp. 400 °C
 55
@Treatment Temp. 500 °C
 56
@Treatment Temp. 550.0 °C
Tensile Strength 205 ksi
@Temperature -5.56 °C
45 HRC
 250 ksi
@Temperature -5.56 °C
50 HRC
 290 ksi
@Temperature -5.56 °C
55 HRC
Tensile Strength, Yield 180 ksi
@Temperature 22.0 °C
45 HRC
 210 ksi
@Temperature 22.0 °C
50 HRC
 225 ksi
@Temperature 22.0 °C
55 HRC
Elongation at Yield 8.0 %
@Temperature 22.0 °C
55 HRC
 10 %
@Temperature 22.0 °C
50 HRC
 12 %
@Temperature 22.0 °C
45 HRC
 
Thermal PropertiesOriginal ValueComments
CTE, linear 6.20 µin/in-°F
@Temperature 21.1 - 93.3 °C
 6.40 µin/in-°F
@Temperature 21.1 - 204 °C
 6.40 µin/in-°F
@Temperature 21.1 - 288 °C
Thermal Conductivity 156 BTU-in/hr-ft²-°F
@Temperature 93.3 °C
 160 BTU-in/hr-ft²-°F
@Temperature 149 °C
 163 BTU-in/hr-ft²-°F
@Temperature 204 °C
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 1400 - 1470 °FSoft; Cooling: Furnace 20°F/hour to 1200 °F/ Then air cooled; < 230 HB
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.42 %
Chromium, Cr 13 %
Iron, Fe 86.58 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI Type P20 Mold Steel (UNS T51620)
Industeel CLC 1.2316 Prehardened (300HB) and Corrosion Resistant Mold Steel
420 Stainless Steel
Schmolz + Bickenbach Formadur® 2316/2316 ESR Plastic Mold Steel
LG Chemical LI911 ASA

NSCHMO006 / 125879

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.