MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

SABIC LNP™ LUBRICOMP™ ZX05506 PPE+PS (Americas)  (Unverified Data**)
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene + Polyphenylene Ether, Carbon Filler

Material Notes: LNP LUBRICOMP* ZX05506 is a compound based on PPE+PS Blend resin containing 15% Graphite Powder, 20% PTFE. Added feature of this material is: Wear Resistant.

Information provided by Sabic

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.35 g/cc0.0488 lb/in³ASTM D792
 1.35 g/cc0.0488 lb/in³ISO 1183
Moisture Absorption 0.0500 %0.0500 %(23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow  0.0050 cm/cm
@Time 86400 sec
0.0050 in/in
@Time 24.0 hour
ASTM D955
 0.0050 cm/cm
@Time 86400 sec
0.0050 in/in
@Time 24.0 hour
ISO 294
Linear Mold Shrinkage, Transverse  0.0050 cm/cm
@Time 86400 sec
0.0050 in/in
@Time 24.0 hour
ASTM D955
 0.0054 cm/cm
@Time 86400 sec
0.0054 in/in
@Time 24.0 hour
ISO 294
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 50.0 MPa7250 psiISO 527
 52.0 MPa7540 psiASTM D638
Elongation at Break 2.4 %2.4 %ASTM D638
 2.5 %2.5 %ISO 527
Tensile Modulus 4.89 GPa709 ksi50 mm/min; ASTM D638
 4.91 GPa712 ksi1mm/min; ISO 527
Flexural Strength 94.0 MPa13600 psiISO 178
 99.0 MPa14400 psiASTM D790
Flexural Modulus 4.96 GPa719 ksiASTM D790
 5.37 GPa779 ksiISO 178
Izod Impact, Notched 0.320 J/cm0.599 ft-lb/inASTM D256
Izod Impact, Unnotched 1.76 J/cm3.30 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 2.00 kJ/m²0.952 ft-lb/in²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 12.0 kJ/m²5.71 ft-lb/in²80*10*4; ISO 180/1U
Impact Test 1.00 J0.738 ft-lbMultiaxial Impact; ISO 6603
Instrumented Impact Energy at Peak 3.00 J2.21 ft-lbASTM D3763
Coefficient of Friction, Dynamic 0.340.34ASTM D3702 Modified: Manual
Coefficient of Friction, Static 0.340.34ASTM D3702 Modified: Manual
K (wear) Factor 351 x 10-8 mm³/N-M174 x 10-10 in³-min/ft-lb-hrWasher [10^-10 in^5-min/ft-lb-hr]; ASTM D3702 Modified: Manual
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 126 °C259 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 121 °C
@Thickness 3.20 mm
250 °F
@Thickness 0.126 in
unannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Zone 1 275 - 290 °C527 - 554 °F
Zone 2 290 - 300 °C554 - 572 °F
Zone 3 300 - 310 °C572 - 590 °F
Melt Temperature 300 - 305 °C572 - 581 °F
Mold Temperature 80.0 - 110 °C176 - 230 °F
Drying Temperature 120 °C248 °F
Dry Time 4.00 hour4.00 hour
Back Pressure 0.200 - 0.300 MPa29.0 - 43.5 psi
Screw Speed 30 - 60 rpm30 - 60 rpm

**
This data sheet is not an active part of MatWeb and the information on it should not be considered reliable.
Inactive data sheets have usually been replaced with newer information on the same material. If this is the case, you can find the active data sheet by using any of our search tools, including the Quick Search box in the upper part of this page.
If you are unable to locate an active data sheet for this material, then this material is likely discontinued, although various other reasons may be behind its removal. In any event, do not rely on the information on this page to be accurate or maintained.
You may have reached this data sheet through an outdated bookmark or link. Please update your bookmark accordingly. We apologize if you have accessed this page through MatWeb’s usual search tools.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABI30437 / 228808

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.