MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Huntsman IROGRAN® A 95 E 4861 Polyester-Based TPU-Injection Extrusion Grade
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane TPE; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Polyester Grade

Material Notes: Introduction: IROGRAN A95 4861 is a high performance polyester based thermoplastic polyurethane intended for extrusion applications. IROGRAN A95E 4861 is part of the HUNTSMAN technical extrusion product range and offers a specially designed, flexible material with a broad processing window particularly suitable for the preparation of extruded films.

Performance Features:

  • Excellent hydrolysis resistance
  • High crystallization rate
  • Good low temperature flexibility
  • Good processability

Information provided by Huntsman

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.22 g/cc0.0441 lb/in³ASTM D792
Linear Mold Shrinkage 0.011 cm/cm0.011 in/inASTM D995
Melt Index of Compound 45 g/10 min
@Load 21.6 kg,
Temperature 215 °C
45 g/10 min
@Load 47.6 lb,
Temperature 419 °F
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 9696ASTM D2240
Hardness, Shore D 5454ASTM D2240
Tensile Strength at Break 55.0 MPa7980 psiDIN 53504
Elongation at Break 590 %590 %ASTM D412
100% Modulus 12.0 MPa
@Strain 100 %
1740 psi
@Strain 100 %
DIN 53504
300% Modulus 26.0 MPa
@Strain 300 %
3770 psi
@Strain 300 %
DIN 53504
Rebound 35 %35 %Bayshore; ASTM D2632
Tear Strength 145 kN/m830 pliASTM D624
Abrasion 2727[mm3]; ISO 4649
Compression Set  26 %
@Temperature 23.0 °C,
Time 252000 sec
26 %
@Temperature 73.4 °F,
Time 70.0 hour
ASTM D395
 46 %
@Temperature 70.0 °C,
Time 86400 sec
46 %
@Temperature 158 °F,
Time 24.0 hour
ASTM D395
 
Thermal PropertiesMetricEnglishComments
Melting Point 190 - 200 °C374 - 392 °FHuntsman/TMA
 
Processing PropertiesMetricEnglishComments
Feed Temperature 25.0 - 40.0 °C77.0 - 104 °FExtrusion
Front Barrel Temperature 200 - 215 °C392 - 419 °FExtrusion
Nozzle Temperature 200 - 215 °C392 - 419 °FExtrusion
Adapter Temperature 200 - 215 °C392 - 419 °FExtrusion
Die Temperature 200 - 215 °C392 - 419 °FExtrusion

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Huntsman IROGRAN® A 92 E 4738 Polyester-Based TPU-Injection Extrusion Grade
Huntsman IROGRAN® A 92 E 4694 Polyester-Based TPU-Injection Extrusion Grade
Huntsman IROGRAN® A 95 E 4813 Polyester-Based TPU-High Performance Grade
Huntsman IROGRAN® A 98 E 4735 Polyester-Based TPU-Injection Extrusion Grade
Huntsman IROGRAN® A 98 H 4661 Polyester-Based TPU-Injection Molding Grade

PHU9921 / 150381

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.