MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

(Viewing data as-entered. Click here to return)
Evonik VESTAMID® LXM4 Nylon 12, 4% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12); Nylon 12, 20% Glass Fiber Filled

Material Notes: VESTAMID LXM4 is a semi-crystalline, heat- and UV-stabilized compound based on PA12 with a glass fiber content of 4 %. In general, the material is suitable for sport and lifestyle applications and specifically for shoe soles that require good fatigue performance and bonding ability to TPUs. VESTAMID LXM4 only absorbs small amounts of water. Therefore, components made of this material have excellent dimensional accuracy under changing ambient humidity. The material provides a wide processing window in the injection molding process with a high ratio of flow length to wall thickness. The use of colorants can change the property values. VESTAMID® LXM4 is supplied as cylindrical granules ready for processing, in moisture barrier bags. Inside the original and undamaged packaging the product has a shelf life of at least two years when stored in dry rooms at temperatures not exceeding 30°C.
Dry properties listed below
Industrial Sector: Sports and Lifestyle
Processing: Injection molding
Delivery form: Pellets, Granules
Optics: Translucent
Resistance to: Heat (thermal stability), UV / light / weathering
Electrical: Insulating
Additives: Glass fibers
Applications: General purpose
Special Characteristics: Semi-crystalline, Light-stabilized, U.V. stabilized
Color: Natural color
Additives: Light stabilizer, Heat stabilizer
Delivery form: Cylindrical pellets
Chemical Resistance: General chemical resistance

Information provided by Evonik.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.03 g/ccISO 1183
Water Absorption 0.260 %Sim to ISO 62
Moisture Absorption 0.170 %Sim to ISO 62
Linear Mold Shrinkage, Flow 0.00900 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.00600 cm/cmISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 73.0ISO 7619-1
Tensile Strength at Break 39.0 MPaISO 527
Tensile Strength 48.0 MPaISO 527
Tensile Strength, Yield 48.0 MPaISO 527
Elongation at Break 18.3 %Nominal; ISO 527
 18.8 %ISO 527
Elongation at Yield 5.60 %ISO 527
Tensile Modulus 1600 MPaISO 527
Flexural Strength 44.0 MPaat conv. Deflection; ISO 178
 60.0 MPaISO 178
Flexural Modulus 1320 MPaISO 178
Flexural Strain at Break 7.50 %at flexural strength; ISO 178
Charpy Impact Unnotched 130 kJ/m²
@Temperature 23.0 °C
Type of failure: C; ISO 179/1eU
 131 kJ/m²
@Temperature -30.0 °C
Type of failure: C; ISO 179/1eU
Charpy Impact, Notched 6.00 kJ/m²
@Temperature -30.0 °C
Type of failure: C; ISO 179/1eA
 10.0 kJ/m²
@Temperature 23.0 °C
Type of failure: C; ISO 179/1eA
 
Thermal PropertiesOriginal ValueComments
Melting Point 180 °CISO 11357-1/-3
 
Processing PropertiesOriginal ValueComments
Melt Temperature 240 °C
Mold Temperature 60.0 °C
 
Descriptive Properties
Color-0.4Color a, CIE
 3.1Color b, CIE
 64.4Color L, CIE
 Natural Color

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PEVONIK7931 / 325063

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.