MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Extreme Materials from MCAM
Visit Mitsubishi Chemical Advanced Materials for Extreme Materials - high performance plastic machining stock engineered to replace metals such as nickel alloys or stainless steel.

Haynes HR-160® alloy, hot rolled and solution annealed plate
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Outstanding resistance to various forms of high-temperature corrosion attack, excellent resistance to sulfidation and chloride attack in both reducing and oxidizing atmospheres. Excellent forming and welding characteristics. Applications include a variety of fabricated components in municipal, industrial, hazardous, and nuclear waste heat recovery systems. Also suitable for utility boilers, sulfur plants, high-temperature furnaces, kilns, calciners, resource recovery units, cement kilns, pulp and paper recovery boilers, coal gasification systems, and fluidized-bed-combustion systems.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: UNS N12160, ASTM B435, ASTM B366, DIN No.2.4880
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.08 g/cc0.292 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 767 MPa111000 psi
 30.0 MPa
@Temperature 1204 °C
4350 psi
@Temperature 2199 °F
 41.0 MPa
@Temperature 1149.0 °C
5950 psi
@Temperature 2100.2 °F
 74.0 MPa
@Temperature 1093 °C
10700 psi
@Temperature 1999 °F
 140 MPa
@Temperature 982 °C
20300 psi
@Temperature 1800 °F
 264 MPa
@Temperature 871 °C
38300 psi
@Temperature 1600 °F
 428 MPa
@Temperature 760 °C
62100 psi
@Temperature 1400 °F
 523 MPa
@Temperature 649 °C
75900 psi
@Temperature 1200 °F
 564 MPa
@Temperature 538 °C
81800 psi
@Temperature 1000 °F
 605 MPa
@Temperature 427 °C
87700 psi
@Temperature 801 °F
 634 MPa
@Temperature 316 °C
92000 psi
@Temperature 601 °F
 675 MPa
@Temperature 204 °C
97900 psi
@Temperature 399 °F
 717 MPa
@Temperature 93.0 °C
104000 psi
@Temperature 199 °F
Tensile Strength, Yield 314 MPa
@Strain 0.2 %
45500 psi
@Strain 0.2 %
 11.0 MPa
@Strain 0.2 %,
Temperature 1204 °C
1600 psi
@Strain 0.2 %,
Temperature 2199 °F
 16.0 MPa
@Strain 0.2 %,
Temperature 1149 °C
2320 psi
@Strain 0.2 %,
Temperature 2100 °F
 34.0 MPa
@Strain 0.2 %,
Temperature 1093 °C
4930 psi
@Strain 0.2 %,
Temperature 1999 °F
 74.0 MPa
@Strain 0.2 %,
Temperature 982 °C
10700 psi
@Strain 0.2 %,
Temperature 1800 °F
 152 MPa
@Strain 0.2 %,
Temperature 871 °C
22000 psi
@Strain 0.2 %,
Temperature 1600 °F
 170 MPa
@Strain 0.2 %,
Temperature 760 °C
24700 psi
@Strain 0.2 %,
Temperature 1400 °F
 176 MPa
@Strain 0.2 %,
Temperature 538 °C
25500 psi
@Strain 0.2 %,
Temperature 1000 °F
 177 MPa
@Strain 0.2 %,
Temperature 649 °C
25700 psi
@Strain 0.2 %,
Temperature 1200 °F
 179 MPa
@Strain 0.2 %,
Temperature 427 °C
26000 psi
@Strain 0.2 %,
Temperature 801 °F
 190 MPa
@Strain 0.2 %,
Temperature 316 °C
27600 psi
@Strain 0.2 %,
Temperature 601 °F
 233 MPa
@Strain 0.2 %,
Temperature 204 °C
33800 psi
@Strain 0.2 %,
Temperature 399 °F
 279 MPa
@Strain 0.2 %,
Temperature 93.0 °C
40500 psi
@Strain 0.2 %,
Temperature 199 °F
Elongation at Break 68 %68 %in 34.0 mm
 69 %
@Temperature 93.0 °C
69 %
@Temperature 199 °F
in 34.0 mm
 70 %
@Temperature 649 °C
70 %
@Temperature 1200 °F
in 34.0 mm
 71 %
@Temperature 204 °C
71 %
@Temperature 399 °F
in 34.0 mm
 73 %
@Temperature 760 °C
73 %
@Temperature 1400 °F
in 34.0 mm
 74 %
@Temperature 316 °C
74 %
@Temperature 601 °F
in 34.0 mm
 76 %
@Temperature 427 °C
76 %
@Temperature 801 °F
in 34.0 mm
 76 %
@Temperature 538 °C
76 %
@Temperature 1000 °F
in 34.0 mm
 85 %
@Temperature 871 °C
85 %
@Temperature 1600 °F
in 34.0 mm
 88 %
@Temperature 1093 °C
88 %
@Temperature 1999 °F
in 34.0 mm
 90 %
@Temperature 982 °C
90 %
@Temperature 1800 °F
in 34.0 mm
 110 %
@Temperature 1204 °C
110 %
@Temperature 2199 °F
in 34.0 mm
 113 %
@Temperature 1149.0 °C
113 %
@Temperature 2100.2 °F
in 34.0 mm
Reduction of Area 73 %73 %
 64 %
@Temperature 760 °C
64 %
@Temperature 1400 °F
 67 %
@Temperature 649 °C
67 %
@Temperature 1200 °F
 68 %
@Temperature 427 °C
68 %
@Temperature 801 °F
 69 %
@Temperature 538 °C
69 %
@Temperature 1000 °F
 70 %
@Temperature 316 °C
70 %
@Temperature 601 °F
 74 %
@Temperature 93.0 °C
74 %
@Temperature 199 °F
 74 %
@Temperature 204 °C
74 %
@Temperature 399 °F
 84 %
@Temperature 871 °C
84 %
@Temperature 1600 °F
 94 %
@Temperature 1204 °C
94 %
@Temperature 2199 °F
 94 %
@Temperature 1149.0 °C
94 %
@Temperature 2100.2 °F
 98 %
@Temperature 982 °C
98 %
@Temperature 1800 °F
 98 %
@Temperature 1093 °C
98 %
@Temperature 1999 °F
Modulus of Elasticity 211 GPa30600 ksi
 137 GPa
@Temperature 980 °C
19900 ksi
@Temperature 1800 °F
 145 GPa
@Temperature 925 °C
21000 ksi
@Temperature 1700 °F
 150 GPa
@Temperature 870 °C
21800 ksi
@Temperature 1600 °F
 154 GPa
@Temperature 815 °C
22300 ksi
@Temperature 1500 °F
 158 GPa
@Temperature 760 °C
22900 ksi
@Temperature 1400 °F
 163 GPa
@Temperature 705 °C
23600 ksi
@Temperature 1300 °F
 168 GPa
@Temperature 650 °C
24400 ksi
@Temperature 1200 °F
 173 GPa
@Temperature 595 °C
25100 ksi
@Temperature 1100 °F
 177 GPa
@Temperature 540 °C
25700 ksi
@Temperature 1000 °F
 180 GPa
@Temperature 480 °C
26100 ksi
@Temperature 896 °F
 183 GPa
@Temperature 425 °C
26500 ksi
@Temperature 797 °F
 187 GPa
@Temperature 370 °C
27100 ksi
@Temperature 698 °F
 192 GPa
@Temperature 315 °C
27800 ksi
@Temperature 599 °F
 197 GPa
@Temperature 260 °C
28600 ksi
@Temperature 500 °F
 201 GPa
@Temperature 205 °C
29200 ksi
@Temperature 401 °F
 204 GPa
@Temperature 150 °C
29600 ksi
@Temperature 302 °F
 208 GPa
@Temperature 90.0 °C
30200 ksi
@Temperature 194 °F
 210 GPa
@Temperature 40.0 °C
30500 ksi
@Temperature 104 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0001112 ohm-cm0.0001112 ohm-cm
 0.0001231 ohm-cm
@Temperature 700 °C
0.0001231 ohm-cm
@Temperature 1290 °F
 0.0001238 ohm-cm
@Temperature 800 °C
0.0001238 ohm-cm
@Temperature 1470 °F
 0.0001245 ohm-cm
@Temperature 900 °C
0.0001245 ohm-cm
@Temperature 1650 °F
 0.0001252 ohm-cm
@Temperature 1000 °C
0.0001252 ohm-cm
@Temperature 1830 °F
 0.0001259 ohm-cm
@Temperature 1100 °C
0.0001259 ohm-cm
@Temperature 2010 °F
 0.0001267 ohm-cm
@Temperature 1200 °C
0.0001267 ohm-cm
@Temperature 2190 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  13.0 µm/m-°C
@Temperature 25.0 - 95.0 °C
7.22 µin/in-°F
@Temperature 77.0 - 203 °F
 13.7 µm/m-°C
@Temperature 25.0 - 205 °C
7.61 µin/in-°F
@Temperature 77.0 - 401 °F
 14.0 µm/m-°C
@Temperature 25.0 - 315 °C
7.78 µin/in-°F
@Temperature 77.0 - 599 °F
 14.4 µm/m-°C
@Temperature 25.0 - 425 °C
8.00 µin/in-°F
@Temperature 77.0 - 797 °F
 14.9 µm/m-°C
@Temperature 25.0 - 540 °C
8.28 µin/in-°F
@Temperature 77.0 - 1000 °F
 15.5 µm/m-°C
@Temperature 25.0 - 600 °C
8.61 µin/in-°F
@Temperature 77.0 - 1110 °F
 15.7 µm/m-°C
@Temperature 25.0 - 700 °C
8.72 µin/in-°F
@Temperature 77.0 - 1290 °F
 16.6 µm/m-°C
@Temperature 25.0 - 800 °C
9.22 µin/in-°F
@Temperature 77.0 - 1470 °F
 17.1 µm/m-°C
@Temperature 25.0 - 900 °C
9.50 µin/in-°F
@Temperature 77.0 - 1650 °F
Specific Heat Capacity 0.462 J/g-°C0.110 BTU/lb-°F
 0.653 J/g-°C
@Temperature 700 °C
0.156 BTU/lb-°F
@Temperature 1290 °F
 0.672 J/g-°C
@Temperature 800 °C
0.161 BTU/lb-°F
@Temperature 1470 °F
 0.689 J/g-°C
@Temperature 900 °C
0.165 BTU/lb-°F
@Temperature 1650 °F
 0.719 J/g-°C
@Temperature 1100 °C
0.172 BTU/lb-°F
@Temperature 2010 °F
 0.732 J/g-°C
@Temperature 1200 °C
0.175 BTU/lb-°F
@Temperature 2190 °F
 0.784 J/g-°C
@Temperature 1000 °C
0.187 BTU/lb-°F
@Temperature 1830 °F
Thermal Conductivity 10.9 W/m-K75.6 BTU-in/hr-ft²-°F
 21.8 W/m-K
@Temperature 600 °C
151 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 24.7 W/m-K
@Temperature 700 °C
171 BTU-in/hr-ft²-°F
@Temperature 1290 °F
 26.1 W/m-K
@Temperature 800 °C
181 BTU-in/hr-ft²-°F
@Temperature 1470 °F
 26.9 W/m-K
@Temperature 900 °C
187 BTU-in/hr-ft²-°F
@Temperature 1650 °F
 28.7 W/m-K
@Temperature 1000 °C
199 BTU-in/hr-ft²-°F
@Temperature 1830 °F
 31.1 W/m-K
@Temperature 1100 °C
216 BTU-in/hr-ft²-°F
@Temperature 2010 °F
 32.9 W/m-K
@Temperature 1200 °C
228 BTU-in/hr-ft²-°F
@Temperature 2190 °F
Melting Point 1293 - 1370 °C2359 - 2500 °F
Solidus 1293 °C2359 °F
Liquidus 1370 °C2500 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.050 %0.050 %
Chromium, Cr 28 %28 %
Cobalt, Co 30 %30 %
Iron, Fe <= 3.5 %<= 3.5 %
Manganese, Mn 0.50 %0.50 %
Molybdenum, Mo <= 1.0 %<= 1.0 %
Nickel, Ni 37 %37 %
Niobium, Nb (Columbium, Cb) <= 1.0 %<= 1.0 %
Silicon, Si 2.75 %2.75 %
Titanium, Ti 0.50 %0.50 %
Tungsten, W <= 1.0 %<= 1.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Haynes Hastelloy® X alloy, sheet
Special Metals INCONEL® Alloy C-276
446 Stainless Steel, Annealed Bar
Haynes Multimet® alloy, 6.15 mm hot-rolled bar, 25% cold reduction
Special Metals INCONEL® Alloy 600

NH16AA / 16323

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.