MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

LNP Lubricomp® YL-4530 Thermoplastic Polyester Elastomer, Silicone + PTFE Lubricant  (discontinued **)
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyester, TP

Material Notes:
  • Features: Lubricated
  • Forms: Pellets
  • Processing Method: Injection Molding

Information provided by LNP, a GE Plastics Company.

This data sheet is labeled Discontinued; however many LNP grades are still active under new names instituted after the SABIC purchase.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.27 g/cc1.27 g/ccMethod A; ASTM D792
Density 1.27 g/cc0.0459 lb/in³ISO 1183
Water Absorption 0.30 %0.30 %at 24 hrs; ASTM D570
Linear Mold Shrinkage 0.021 cm/cm0.021 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.020 cm/cm0.020 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 13.8 MPa2000 psiASTM D638
Elongation at Yield 54 %54 %ASTM D638
Tensile Modulus 0.207 GPa30.0 ksiASTM D638
Flexural Modulus 0.262 GPa38.0 ksiASTM D790
Izod Impact, Notched 2.40 J/cm
@Thickness 3.18 mm
4.50 ft-lb/in
@Thickness 0.125 in
ASTM D256
Izod Impact, Unnotched NB
@Thickness 3.18 mm
NB
@Thickness 0.125 in
ASTM D256
Izod Impact, Notched (ISO) 27.1 kJ/m²12.9 ft-lb/in²ISO 180
Izod Impact, Unnotched (ISO) NBNBISO 180
Falling Dart Impact 27.7 J20.4 ft-lbASTM D3763
Instrumented Impact Total Energy 26.9 J19.8 ft-lbMulti-Axial Instrumented Impact Energy; ISO 6603-2
Coefficient of Friction, Dynamic 0.480.48vs. Steel - @ 40 psi, 50 ft/min, tested in accordance with LNP WI-0687; ASTM D1894
Coefficient of Friction, Static 0.460.46vs. Steel @ 40 psi, in accordance with LNP WI-0687; ASTM D1894
K (wear) Factor 10.1 x 10-8 mm³/N-M5.00 x 10-10 in³-min/ft-lb-hr40psi, 50ft/min; tested in accordance with LNP WI-0687
 
Thermal PropertiesMetricEnglishComments
CTE, linear 110 µm/m-°C
@Temperature 20.0 °C
61.1 µin/in-°F
@Temperature 68.0 °F
TMA; ASTM E831
CTE, linear, Transverse to Flow 180 µm/m-°C
@Temperature 20.0 °C
100 µin/in-°F
@Temperature 68.0 °F
TMA; ASTM E831
Deflection Temperature at 1.8 MPa (264 psi) 47.2 °C117 °FUnannealed; ASTM D648
 
Processing PropertiesMetricEnglishComments
Melt Temperature 216 - 238 °C421 - 460 °F
Mold Temperature 23.9 - 51.7 °C75.0 - 125 °F
Drying Temperature 82.2 °C180 °F
Dry Time 4 hour4 hour
Moisture Content 0.10 %0.10 %Suggested
Back Pressure 0.172 - 0.345 MPa24.9 - 50.0 psi

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Thermoplastic Polyurethane, Elastomer, Polyester Grade

PZLNP1209 / 51291

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.