MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Pressure Seal 8648 Fluorinated Hydrocarbon
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 8648 is a 60 durometer black colored Viton A elastomer, it is formulated with FDA approved materials. It exhibits excellent resistance to heat, compression set and petroleum based oils.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 2 HK 610 A1-10 B37 B38 EO78 F15; 4 HK 610 A1-11 B38 EO78; 6 HK 610 A1-10 A1-11 B31 EO88 F15
3A Sanitary Standards Class I, II, III, IV.

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.84 g/cc1.84 g/cc
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6565
 59
@Treatment Temp. 200 °C,
Time 252000 sec
59
@Treatment Temp. 392 °F,
Time 70.0 hour
Stauffer Blend 7700
 61
@Treatment Temp. 200 °C,
Time 252000 sec
61
@Treatment Temp. 392 °F,
Time 70.0 hour
Service Fluid 101
 64
@Treatment Temp. 23.0 °C,
Time 252000 sec
64
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel C
 65
@Treatment Temp. 150 °C,
Time 252000 sec
65
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #1
 65
@Treatment Temp. 150 °C,
Time 252000 sec
65
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #3
 65
@Treatment Temp. 250 °C,
Time 252000 sec
65
@Treatment Temp. 482 °F,
Time 70.0 hour
Heat Aged
 65
@Treatment Temp. 100 °C,
Time 252000 sec
65
@Treatment Temp. 212 °F,
Time 70.0 hour
Distilled water aged
 67
@Treatment Temp. 275 °C,
Time 252000 sec
67
@Treatment Temp. 527 °F,
Time 70.0 hour
Heat Aged
Tensile Strength 9.680 MPa1404 psi
 6.25 MPa
@Treatment Temp. 23.0 °C,
Time 252000 sec
907 psi
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel C
 7.2312 MPa
@Treatment Temp. 200 °C,
Time 252000 sec
1048.8 psi
@Treatment Temp. 392 °F,
Time 70.0 hour
Stauffer Blend 7700
 8.0345 MPa
@Treatment Temp. 200 °C,
Time 252000 sec
1165.3 psi
@Treatment Temp. 392 °F,
Time 70.0 hour
Service Fluid 101
 9.6223 MPa
@Treatment Temp. 275 °C,
Time 252000 sec
1395.6 psi
@Treatment Temp. 527 °F,
Time 70.0 hour
Heat Aged
 9.8547 MPa
@Treatment Temp. 150 °C,
Time 252000 sec
1429.3 psi
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #3
 10.097 MPa
@Treatment Temp. 250 °C,
Time 252000 sec
1464.4 psi
@Treatment Temp. 482 °F,
Time 70.0 hour
Heat Aged
 11.307 MPa
@Treatment Temp. 150 °C,
Time 252000 sec
1639.9 psi
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #1
Elongation, Ultimate 230 %230 %
 180 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
180 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
ASTM Reference Fuel C
 204 %
@Treatment Temp. 250 °C,
Time 252000 sec
204 %
@Treatment Temp. 482 °F,
Time 70.0 hour
Heat Aged
 206.1 %
@Treatment Temp. 200 °C,
Time 252000 sec
206.1 %
@Treatment Temp. 392 °F,
Time 70.0 hour
Stauffer Blend 7700
 223 %
@Treatment Temp. 200 °C,
Time 252000 sec
223 %
@Treatment Temp. 392 °F,
Time 70.0 hour
Service Fluid 101
 224 %
@Treatment Temp. 150 °C,
Time 252000 sec
224 %
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #3
 224.9 %
@Treatment Temp. 275 °C,
Time 252000 sec
224.9 %
@Treatment Temp. 527 °F,
Time 70.0 hour
Heat Aged
 238.9 %
@Treatment Temp. 150 °C,
Time 252000 sec
238.9 %
@Treatment Temp. 302 °F,
Time 70.0 hour
ASTM Oil #1
100% Modulus 2.48 MPa360 psi
Tear Strength 14.4 kN/m82.0 pliDie B
 16.5 kN/m94.0 pliDie C
Compression Set  4.6 %
@Treatment Temp. 175 °C,
Time 79200 sec
4.6 %
@Treatment Temp. 347 °F,
Time 22.0 hour
Plied
 8.6 %
@Treatment Temp. 200 °C,
Time 79200 sec
8.6 %
@Treatment Temp. 392 °F,
Time 22.0 hour
Plied
 9.4 %
@Treatment Temp. 23.0 °C,
Time 79200 sec
9.4 %
@Treatment Temp. 73.4 °F,
Time 22.0 hour
Plied
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -26.1 °C-15.0 °F
Shrinkage  0.60 %
@Treatment Temp. 150 °C,
Time 252000 sec
0.60 %
@Treatment Temp. 302 °F,
Time 70.0 hour
Volume, ASTM Oil #1
 0.90 %
@Treatment Temp. 100 °C,
Time 252000 sec
0.90 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Volume, Distilled water aged
 2.2 %
@Treatment Temp. 150 °C,
Time 252000 sec
2.2 %
@Treatment Temp. 302 °F,
Time 70.0 hour
Volume, ASTM Oil #3
 3.5 %
@Treatment Temp. 23.0 °C,
Time 252000 sec
3.5 %
@Treatment Temp. 73.4 °F,
Time 70.0 hour
Volume, ASTM Reference Fuel C
 10.2 %
@Treatment Temp. 200 °C,
Time 252000 sec
10.2 %
@Treatment Temp. 392 °F,
Time 70.0 hour
Volume, Service Fluid 100
 18.4 %
@Treatment Temp. 200 °C,
Time 252000 sec
18.4 %
@Treatment Temp. 392 °F,
Time 70.0 hour
Volume, Stauffer Blend 7700
 
Descriptive Properties
ColorBlack

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PPRESL098 / 318308

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.