MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Uranium, U; Beta-Annealed
Categories: Metal; Nonferrous Metal; Pure Element

Material Notes: Beta-annealed applies only to tensile and/or hardness values; other property values are typical of the element.

Two other pure U sample preps are in MatWeb.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 19.07 g/cc0.6889 lb/in³
 
Chemical PropertiesMetricEnglishComments
Atomic Mass 238.0289238.02891995
Atomic Number 9292
Thermal Neutron Cross Section 694 barns/atom694 barns/atom
X-ray Absorption Edge 0.10775 Å0.10775 ÅK
 0.56974 Å0.56974 ÅLI
 0.59186 Å0.59186 ÅLII
 0.72225 Å0.72225 ÅLIII
Electrode Potential -1.40 V-1.40 V
Electronegativity 1.71.7Pauling
Ionic Radius 0.800 Å0.800 ÅCrystal Ionic Radius for Valence +6
 0.970 Å0.970 ÅCrystal Ionic Radius for Valence +4
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 185185Converted from Vickers for 3000 kg load/10 mm ball Brinell test. Unspecified heat treatment.
Hardness, Rockwell A 5555Converted from Vickers. Unspecified heat treatment.
Hardness, Rockwell B 9090Converted from Vickers. Unspecified heat treatment.
Hardness, Rockwell C 1010Converted from Vickers. Unspecified heat treatment.
Hardness, Vickers 190190Unspecified heat treatment.
Tensile Strength, Ultimate 615 MPa89200 psi
Modulus of Elasticity 190 GPa27600 ksi
Poissons Ratio 0.220.22
Shear Modulus 77.9 GPa11300 ksiCalculated
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000300 ohm-cm0.0000300 ohm-cm
Magnetic Susceptibility 0.000001760.00000176cgs/g
Critical Superconducting Temperature 0.400 - 2.40 K0.400 - 2.40 K2.4-0.4 K from 1.0-8.5 GPa pressure
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 50.0 J/g21.5 BTU/lb
CTE, linear 19.0 µm/m-°C
@Temperature 20.0 - 100 °C
10.6 µin/in-°F
@Temperature 68.0 - 212 °F
Specific Heat Capacity 0.1156 J/g-°C0.02763 BTU/lb-°F
Thermal Conductivity 26.8 W/m-K186 BTU-in/hr-ft²-°F
Melting Point 1132.3 °C2070.1 °F
Boiling Point 4131 °C7468 °F
 
Optical PropertiesMetricEnglishComments
Emissivity (0-1) 0.540.54unoxidized total
Reflection Coefficient, Visible (0-1) 0.7350.735spectral 660 nm
 
Component Elements PropertiesMetricEnglishComments
Uranium, U 100 %100 %
 
Descriptive Properties
CAS Number7440-61-1

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Uranium, U; Wrought Alpha Phase
Uranium, U; Cast
Molybdenum, Mo, Annealed
Platinum, Pt, Thermocouple Quality, Annealed
Molybdenum, Mo, Recrystallized

AMEU001 / 119

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.