MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Nylon 12, 50% Glass Fiber Filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12); Nylon 12, 50% Glass Fiber Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Nylon 12, 50% Glass Fiber Filled". Specific grades with glass content between 45% and 54% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 0.00147 - 1.70 g/cc0.0000531 - 0.0614 lb/in³Average value: 1.53 g/cc Grade Count:61
Water Absorption 0.0500 - 1.00 %0.0500 - 1.00 %Average value: 0.510 % Grade Count:54
Moisture Absorption at Equilibrium 0.300 - 0.400 %0.300 - 0.400 %Average value: 0.378 % Grade Count:18
Water Absorption at Saturation 0.700 - 1.00 %0.700 - 1.00 %Average value: 0.812 % Grade Count:34
Linear Mold Shrinkage 0.00100 - 0.00700 cm/cm0.00100 - 0.00700 in/inAverage value: 0.00296 cm/cm Grade Count:58
Linear Mold Shrinkage, Transverse 0.00100 - 0.0100 cm/cm0.00100 - 0.0100 in/inAverage value: 0.00224 cm/cm Grade Count:55
Melt Flow 6.00 - 50.0 g/10 min6.00 - 50.0 g/10 minAverage value: 21.0 g/10 min Grade Count:3
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 82.0 - 88.082.0 - 88.0Average value: 85.3 Grade Count:24
Ball Indentation Hardness 155 - 230 MPa22500 - 33400 psiAverage value: 190 MPa Grade Count:32
Tensile Strength, Ultimate 31.0 - 210 MPa4500 - 30500 psiAverage value: 164 MPa Grade Count:56
 55.0 - 110 MPa
@Temperature 60.0 - 150 °C
7980 - 16000 psi
@Temperature 140 - 302 °F
Average value: 83.8 MPa Grade Count:1
Tensile Strength, Yield 145 - 170 MPa21000 - 24600 psiAverage value: 156 MPa Grade Count:3
Elongation at Break 1.60 - 7.00 %1.60 - 7.00 %Average value: 3.88 % Grade Count:57
 6.20 - 8.60 %
@Temperature 60.0 - 150 °C
6.20 - 8.60 %
@Temperature 140 - 302 °F
Average value: 7.30 % Grade Count:1
Elongation at Yield 3.60 - 6.00 %3.60 - 6.00 %Average value: 4.85 % Grade Count:3
Modulus of Elasticity 4.10 - 20.0 GPa595 - 2900 ksiAverage value: 14.7 GPa Grade Count:56
 3.30 - 6.30 GPa
@Temperature 60.0 - 150 °C
479 - 914 ksi
@Temperature 140 - 302 °F
Average value: 4.75 GPa Grade Count:1
Flexural Yield Strength 214 - 255 MPa31000 - 37000 psiAverage value: 239 MPa Grade Count:5
Flexural Modulus 3.10 - 14.0 GPa450 - 2030 ksiAverage value: 9.15 GPa Grade Count:6
Izod Impact, Notched 1.55 - 96.0 J/cm2.90 - 180 ft-lb/inAverage value: 26.0 J/cm Grade Count:4
Izod Impact, Unnotched 10.7 - 5340 J/cm20.0 - 10000 ft-lb/inAverage value: 42.2 J/cm Grade Count:4
Izod Impact, Notched (ISO) 16.0 - 19.0 kJ/m²
@Temperature -30.0 - -30.0 °C
7.61 - 9.04 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 17.5 kJ/m² Grade Count:2
Izod Impact, Unnotched (ISO) 61.0 - 85.0 kJ/m²
@Temperature -30.0 - -30.0 °C
29.0 - 40.4 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 73.0 kJ/m² Grade Count:2
Charpy Impact Unnotched 6.00 - 10.2 J/cm²28.6 - 48.5 ft-lb/in²Average value: 7.95 J/cm² Grade Count:47
 6.00 - 10.9 J/cm²
@Temperature -40.0 - -30.0 °C
28.6 - 51.9 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 7.88 J/cm² Grade Count:46
Charpy Impact, Notched 1.20 - 2.80 J/cm²5.70 - 13.3 ft-lb/in²Average value: 1.83 J/cm² Grade Count:47
 1.00 - 2.30 J/cm²
@Temperature -40.0 - -30.0 °C
4.76 - 10.9 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 1.52 J/cm² Grade Count:46
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+10 - 2.00e+14 ohm-cm1.00e+10 - 2.00e+14 ohm-cmAverage value: 1.17e+13 ohm-cm Grade Count:38
Surface Resistance 1.00e+11 - 2.30e+14 ohm1.00e+11 - 2.30e+14 ohmAverage value: 6.84e+12 ohm Grade Count:36
Dielectric Strength 17.7 - 55.1 kV/mm450 - 1400 kV/inAverage value: 37.1 kV/mm Grade Count:39
Comparative Tracking Index 60.0 - 600 V60.0 - 600 VAverage value: 585 V Grade Count:35
 
Thermal PropertiesMetricEnglishComments
CTE, linear 10.0 - 101 µm/m-°C5.56 - 56.0 µin/in-°FAverage value: 19.9 µm/m-°C Grade Count:37
CTE, linear, Transverse to Flow 70.0 - 121 µm/m-°C38.9 - 67.0 µin/in-°FAverage value: 96.6 µm/m-°C Grade Count:35
Melting Point 175 - 186 °C347 - 367 °FAverage value: 178 °C Grade Count:34
Maximum Service Temperature, Air 80.0 - 160 °C176 - 320 °FAverage value: 126 °C Grade Count:36
Deflection Temperature at 0.46 MPa (66 psi) 115 - 190 °C239 - 374 °FAverage value: 163 °C Grade Count:7
Deflection Temperature at 1.8 MPa (264 psi) 105 - 185 °C221 - 365 °FAverage value: 161 °C Grade Count:40
Deflection Temperature at 8.0 MPa 105 - 160 °C221 - 320 °FAverage value: 132 °C Grade Count:35
Vicat Softening Point 165 - 180 °C329 - 356 °FAverage value: 174 °C Grade Count:4
Glass Transition Temp, Tg 41.0 - 125 °C106 - 257 °FAverage value: 108 °C Grade Count:5
Flammability, UL94 HBHBGrade Count:32
 
Processing PropertiesMetricEnglishComments
Melt Temperature 50.0 - 280 °C122 - 536 °FAverage value: 233 °C Grade Count:4
Mold Temperature 60.0 - 104 °C140 - 220 °FAverage value: 84.2 °C Grade Count:5
Drying Temperature 70.0 - 100 °C158 - 212 °FAverage value: 87.5 °C Grade Count:4

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 12, 20% Glass Fiber Filled
Overview of materials for Nylon 11 with 30% Glass Fiber Filler
Overview of materials for Nylon 11 with 40% Glass Fiber Filler
Overview of materials for Nylon 12, 30% Glass Fiber Filled
Overview of materials for Nylon 12, Carbon Fiber Filled

O2655 / 78076

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.