MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Hexcel® HexMC®-i C/2000/M81 Carbon Epoxy Molding Composite
Categories: Polymer; Thermoset; Carbon Fiber/Thermoset Composite; Epoxy; Epoxy/Carbon Fiber Composite

Material Notes: HexMC®-i is a high-performance carbon moulding compound, specifically designed for compression moulding. The epoxy matrix and high carbon fiber volume content enable components to be molded for a wide range of applications.

Features include:

  • Competitive alternative to lightweight metal alloys (Al, Mg, Ti).
  • Designed for compression molding.
  • Rapid processing cycles.
  • Complex shapes.
  • Moulded-in inserts.
  • No material waste.
  • Elevated temperature performance

Information provided by Hexcel

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.55 g/cc0.0560 lb/in³
Filler Content 57 %57 %Nominal Fiber Volume
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 300 MPa43500 psiASTM D3039
Tensile Modulus 42.0 GPa6090 ksiASTM D3039
Compressive Strength 325 MPa47100 psiEN 6036
Compressive Modulus 35.0 GPa5080 ksiEN 6036
Shear Strength 80.0 MPa11600 psiIn-Line; ASTM D5379
 
Thermal PropertiesMetricEnglishComments
Glass Transition Temp, Tg 165 °C329 °FTypical Cure
 210 °C410 °FTypical Cure + Post Cure 2 hours at 180°C
 
Processing PropertiesMetricEnglishComments
Processing Temperature 180 °C
@Time 1200 sec
356 °F
@Time 0.333 hour
typical
Shelf Life  0.750 Month
@Temperature 23.0 °C
0.750 Month
@Temperature 73.4 °F
 12.0 Month
@Temperature -18.0 °C
12.0 Month
@Temperature -0.400 °F
 
Descriptive Properties
Areal Weight 2000 g/m²
FormRoll

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHEXC703a / 318096

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.