MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

ExxonMobil LD 117.JJ Low Density Polyethylene (LDPE), Film Grade
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Low Density (LDPE); Low Density Polyethylene (LDPE), Film Grade

Material Notes: LD 117 are homopolymer film resins with good clarity and excellent stiffness.  Film made from LD 117 resins can be used in overwrap applications and in push-through type packaging equipment.  With a narrow die gap, film produced from LD 117 resins can be drawn down to 1.0 mil gauge. 

Availability: Latin America, North America.

Additive:  antiblock: 1000ppm; slip: 250ppm; thermal stabilizer: yes. 

Applications:  bread bags, foams, lamination film, co-extrusion films, high performance collation shrink, overwrap film, collation shrink, paper overwrap, diaper back sheet, hygiene packaging, label film.

Information provided by ExxonMobil.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.929 g/cc0.0336 lb/in³ASTM D1505
Melt Flow 1.6 g/10 min
@Load 2.16 kg,
Temperature 190 °C
1.6 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 13.8 MPa2000 psiASTM D882
Film Tensile Strength at Yield, TD 15.9 MPa2300 psiASTM D882
Film Elongation at Break, MD 170 %170 %ASTM D882
Film Elongation at Break, TD 510 %510 %ASTM D882
Puncture Energy 0.339 J0.250 ft-lbExxonMobil Method
Elmendorf Tear Strength MD 190 g190 gASTM D1922
Elmendorf Tear Strength TD 240 g240 gASTM D1922
Dart Drop Test 80.0 g0.176 lbASTM D1709A
Film Tensile Strength at Break, MD 24.8 MPa3600 psiASTM D882
Film Tensile Strength at Break, TD 17.9 MPa2600 psiASTM D882
1% Secant Modulus, MD 317 MPa46000 psiASTM D882
1% Secant Modulus, TD 372 MPa54000 psiASTM D882
 
Thermal PropertiesMetricEnglishComments
Melting Point 116 °C241 °FPeak; ExxonMobil Method
Vicat Softening Point 104 °C219 °FASTM D1525
 
Optical PropertiesMetricEnglishComments
Haze 7.1 %7.1 %ASTM D1003
Gloss 68 %68 %@ 45°; ASTM D2457

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PEX98866 / 238248

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.