Eneos N215SL Nitrile Rubber
Categories:
Polymer
;
Thermoset
;
Rubber or Thermoset Elastomer (TSE)
Material Notes:
Characteristics: Fuel resistance, Oil resistance, Good processability
Application: Oil seal, gasket, various packing, hoses
ENEOS has acquired the elastomer product lines from JSR Corporation.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Specific Gravity
1.01
g/cc
1.01
g/cc
Mooney Viscosity
45
@Temperature 100 °C
45
@Temperature 212 °F
ML1+4
53
@Temperature 100 °C
53
@Temperature 212 °F
ML1+4, Compound (non-vulcanized)
23
@Temperature 125 °C,
Time 57600 sec
23
@Temperature 257 °F,
Time 16.0 hour
Scorch Test, ML1, Compound (non-vulcanized)
Chemical Properties
Metric
English
Comments
Styrene Content
4.0 %
4.0 %
Mechanical Properties
Metric
English
Comments
Hardness, Shore A
81
81
81
81
Compound (vulcanized)
60
@Temperature 40.0 °C,
Time 173000 sec
60
@Temperature 104 °F,
Time 48.0 hour
Fuel Oil B, Compound (non-vulcanized)
73
@Temperature 120 °C,
Time 252000 sec
73
@Temperature 248 °F,
Time 70.0 hour
IRM903, Compound (vulcanized)
83
@Temperature 120 °C,
Time 252000 sec
83
@Temperature 248 °F,
Time 70.0 hour
IRM901, Compound (vulcanized)
84
@Temperature 120 °C,
Time 252000 sec
84
@Temperature 248 °F,
Time 70.0 hour
Air heat Aging, Compound (non-vulcanized)
Tensile Strength
19.2
MPa
2780
psi
19.2
MPa
2780
psi
Compound (vulcanized)
13.632
MPa
@Temperature 40.0 °C,
Time 173000 sec
1977.2
psi
@Temperature 104 °F,
Time 48.0 hour
Fuel Oil B, Compound (non-vulcanized)
17.664
MPa
@Temperature 120 °C,
Time 252000 sec
2562.0
psi
@Temperature 248 °F,
Time 70.0 hour
IRM901, Compound (vulcanized)
19.008
MPa
@Temperature 120 °C,
Time 252000 sec
2756.9
psi
@Temperature 248 °F,
Time 70.0 hour
IRM903, Compound (vulcanized)
19.392
MPa
@Temperature 120 °C,
Time 252000 sec
2812.6
psi
@Temperature 248 °F,
Time 70.0 hour
Air heat Aging, Compound (non-vulcanized)
Elongation at Break
430 %
430 %
430 %
430 %
Compound (vulcanized)
258 %
@Temperature 120 °C,
Time 252000 sec
258 %
@Temperature 248 °F,
Time 70.0 hour
IRM901, Compound (vulcanized)
262.3 %
@Temperature 120 °C,
Time 252000 sec
262.3 %
@Temperature 248 °F,
Time 70.0 hour
Air heat Aging, Compound (non-vulcanized)
326.8 %
@Temperature 120 °C,
Time 252000 sec
326.8 %
@Temperature 248 °F,
Time 70.0 hour
IRM903, Compound (vulcanized)
331.1 %
@Temperature 40.0 °C,
Time 173000 sec
331.1 %
@Temperature 104 °F,
Time 48.0 hour
Fuel Oil B, Compound (non-vulcanized)
100% Modulus
4.70
MPa
682
psi
Compound (vulcanized)
300% Modulus
15.8
MPa
2290
psi
15.8
MPa
2290
psi
Compound (vulcanized)
Resilience
6.0
6.0
[%], Rebound, Compound (vulcanized)
Tear Strength
48.0
kN/m
274
pli
Compound (vulcanized)
Compression Set
22 %
@Temperature 100 °C,
Time 252000 sec
22 %
@Temperature 212 °F,
Time 70.0 hour
Compound (vulcanized)
32 %
@Temperature 120 °C,
Time 252000 sec
32 %
@Temperature 248 °F,
Time 70.0 hour
Compound (vulcanized)
Thermal Properties
Metric
English
Comments
Brittleness Temperature
-8.00
°C
17.6
°F
Descriptive Properties
Acrylonitrile Content (%)
48
Delta;V
100
(%)
16
Fuel Oil B 48 hrs at 40°C, Compound (non-vulcanized)
3
Distilled Water 70 hr at 40°C, Compound (non-vulcanized)
31
Fuel Oil C 48 hrs at 40°C, Compound (non-vulcanized)
-4
IRM901 70 hrs at 120°C, Compound (vulcanized)
-4
IRM903 70 hrs at 120°C, Compound (vulcanized)
48
Fuel Oil C/Ethanol 48 hrs at 40°C, Compound (non-vulcanized)
Extrusion Test
110
80°C, 25 rpm, Die Swell %
362 cm/min
80°C, 25 rpm, Extrusion Length
381 cc/min
80°C, 25 rpm, Extrusion Volume
Flex Test
20
Occurrence(Thousand Times)
3
Growth 2 to 15 mm (Thousand Times)
Flow Rate
115
Q×10
4
, 80°C, 100 kg, Kokahiki Flow tester
JSR Mold Curast Test 160°C, Minutes
2
t
c(10)
8
t
c(90)
Low-Temperature Torsion Test
-1°C
t10
-11°C
t100
Mill Contraction 50°C (%)
25
Ozone Degradability Test
C-3
Static 20% Elongation, 50 ppm 5 Hours at 40°C
C-3
Dynamic 0 to 20% Elongation, 50 ppm 5 Hours at 40°C
Product form
Bale
Product Stain
NS
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
PJSRC8046 / 295362
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.