MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Schmolz + Bickenbach UGIMA® 630 Stainless Steel Bar
Categories: Metal; Ferrous Metal; Stainless Steel; Precipitation Hardening Stainless; T 600 Series Stainless Steel

Material Notes: 630 UGIMA® is an improved machining martensitic precipitation hardenable grade. It is identical to standard type 630 (17-4), except with respect to machinability. The proprietary UGIMA® manufacturing process – developed by Ugitech – results in a product that increases productivity and tool life, and improves the surface finish on all types of machined parts. 630 UGIMA® provides a good combination of high strength corrosion resistance, and is often the best solution of stainless steel when high strength is required. Parts machined from solution treated bar stock should be heat treated or aged prior to use. No further heat treatment of machined parts is required when using 630 UGIMA® is one of the precipitation hardened conditions as specified.

Applications: Fasteners, Shafts, Valve Bodies, Valves, Valve Trim, Fitting, Machined parts, Medical devices, Aircraft components, and Not recommended for vessels containing liquid or gasses at high pressure

Information provided by Schmolz + Bickenbach

Key Words: AISI 630; UNS S17400; EN 10088-3 1.4542, X5CrNiCuNB16.4; ASTM A484; A564; F899; ASME SA-564; API 6A
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.280 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell >= 2771400°F for 2 hrs and 1150°F for 4 hrs
 320 - 340
@Thickness <=25.4 mm
Cold Drawn Bars
 320 - 340
@Thickness >=25.4 mm
Turned Bars
 >= 255
@Treatment Temp. 579.4 °C,
Time 14400 sec
 >= 255
@Treatment Temp. 621 °C,
Time 14400 sec
 >= 331
@Treatment Temp. 551.7 °C,
Time 14400 sec
 >= 388
@Treatment Temp. 482 °C,
Time 3600 sec
Tensile Strength >= 115 ksi1400°F for 2 hrs and 1150°F for 4 hrs
 145 - 165 ksi
@Thickness <=25.4 mm
Cold Drawn Bars
 150 - 170 ksi
@Thickness >=25.4 mm
Turned Bars
 >= 135 ksi
@Treatment Temp. 621 °C,
Time 14400 sec
 >= 145 ksi
@Treatment Temp. 579.4 °C,
Time 14400 sec
 >= 155 ksi
@Treatment Temp. 551.7 °C,
Time 14400 sec
 >= 190 ksi
@Treatment Temp. 482 °C,
Time 3600 sec
Tensile Strength, Yield >= 75.0 ksi1400°F for 2 hrs and 1150°F for 4 hrs
 >= 125 ksi
@Temperature 1075 °C,
Time 14400 sec
 >= 125 ksi
@Temperature 1150 °C,
Time 14400 sec
 >= 155 ksi
@Temperature 1025 °C,
Time 14400 sec
 >= 170 ksi
@Temperature 900 °C,
Time 3600 sec
 115 - 135 ksi
@Strain 0.2 %,
Thickness >=25.4 mm
Turned Bars
 135 - 155 ksi
@Strain 0.2 %,
Thickness <=25.4 mm
Cold Drawn Bars
Elongation at Yield >= 18 %1400°F for 2 hrs and 1150°F for 4 hrs
 >= 0.00 %
@Thickness <=25.4 mm
Cold Drawn Bars
 >= 12 %
@Thickness >=25.4 mm
Turned Bars
 >= 10 %
@Treatment Temp. 482 °C,
Time 3600 sec
 >= 12 %
@Treatment Temp. 551.7 °C,
Time 14400 sec
 >= 13 %
@Treatment Temp. 579.4 °C,
Time 14400 sec
 >= 16 %
@Treatment Temp. 621 °C,
Time 14400 sec
Reduction of Area >= 55 %1400°F for 2 hrs and 1150°F for 4 hrs
 >= 40 %
@Thickness >=25.4 mm
Turned Bars
 >= 50 %
@Thickness <=25.4 mm
Cold Drawn Bars
 >= 34 %
@Treatment Temp. 482 °C,
Time 3600 sec
 >= 45 %
@Treatment Temp. 551.7 °C,
Time 14400 sec
 >= 50 %
@Treatment Temp. 579.4 °C,
Time 14400 sec
 >= 50 %
@Treatment Temp. 621 °C,
Time 14400 sec
Tensile Modulus 28600 ksi
Charpy Impact >= 15.0 ft-lb
@Treatment Temp. 551.7 °C,
Time 14400 sec
 >= 30.0 ft-lb
@Treatment Temp. 579.4 °C,
Time 14400 sec
 >= 30.0 ft-lb
@Treatment Temp. 621 °C,
Time 14400 sec
 >= 55.0 ft-lb
@Treatment Temp. 760 °C,
Time 7200 sec
 >= 55.0 ft-lb
@Treatment Temp. 621 °C,
Time 14400 sec
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000800 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 6.00 µin/in-°F
@Temperature 20.0 - 200 °C
Thermal Conductivity 238 BTU-in/hr-ft²-°F
@Temperature 20.0 °C
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 1900 °F
Hot-Working Temperature 1475 °FStep 1: Slow heating
 1740 - 2190 °FStep 3: Forging range
 2100 - 2190 °FStep 2: More Rapid Heating
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.070 %
Chromium, Cr 15 - 17.5 %
Copper, Cu 3.0 - 4.0 %
Iron, Fe >= 70.46 %
Manganese, Mn <= 1.0 %
Nickel, Ni 3.0 - 5.0 %
Niobium, Nb (Columbium, Cb) 0.15 - 0.45 %
Phosphorus, P <= 0.040 %
Silicon, Si <= 1.0 %
Sulfur, S <= 0.030 %
Tantalum, Ta 0.15 - 0.45 %
 
Descriptive Properties
Corrosion ResistanceAcetic Acid2/4
 Humidity4/4
 NaCl (Saline Mist)3/4
 Nitric Acid3/4
 Sodium Carbonate2/4

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Carpenter Custom 630 (17-Cr-4Ni) Precipitation Hardening Stainless Steel, Condition H 900 (Age-Hardened 482°C/1hr/AC)
AK Steel 17-4 PH® Precipitation Hardening Stainless Steel, Condition H 900
Carpenter Custom 630 (17-Cr-4Ni) Precipitation Hardening Stainless Steel, Annealed
Carpenter Custom 630 (17-Cr-4Ni) Precipitation Hardening Stainless Steel, Condition H 1025 (Heated 552°C)
AK Steel 17-4 PH® Precipitation Hardening Stainless Steel, Condition A

NSCHMO039 / 125912

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.