MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Akro-Plastic Akromid® B3 GF 30 1 XL black (4366) PA 6 Conditioned, 30% Glass Filled, Heat Stabilized
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 30% Glass Fiber Filled; Nylon 6, Heat Stabilized

Material Notes: Description: AKROMID B3 GF 30 1 XL black (4366) is a 30% glass fiber reinforced and heat stabilized polyamide-blend with a greatly reduced density compared to standard PA6 GF 30. Applications are mainly technical components in the automotive and electronic industry, where a weight and cost reduction is required

Additive: Heat Stabilizer

Features:

  • Heat Stabilized
  • Low Density
Uses:
  • Automotive Application
  • Electrical/Electronic Applications
  • Engineering Parts

Information provided by Akro-Plastic GmbH

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.22 g/cc0.0441 lb/in³ISO 1183
Filler Content 30 %30 %ISO 1172
Moisture Absorption 0.80 %
@Temperature 70.0 °C
0.80 %
@Temperature 158 °F
Humidity, 62% RH; ISO 1110
Linear Mold Shrinkage, Flow 0.0037 cm/cm0.0037 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.0085 cm/cm0.0085 in/inISO 294-4
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 100 MPa14500 psi5 [mm/min]; ISO 527-2
Elongation at Break 3.5 %3.5 %5 [mm/min]; ISO 527-2
Tensile Modulus 6.80 GPa986 ksi1 [mm/min]; ISO 527-2
Charpy Impact Unnotched  4.20 J/cm²
@Temperature -30.0 °C
20.0 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
 4.80 J/cm²
@Temperature 23.0 °C
22.8 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  1.30 J/cm²
@Temperature -30.0 °C
6.19 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 1.30 J/cm²
@Temperature 23.0 °C
6.19 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Melting Point 220 °C428 °FDIN EN 11357-1
 
Descriptive Properties
Resistance to Fruit JuicesPass50°C, 100% Conc
Resistance to SpiritsPass100% Conc
Resistance to TolueneFail100% Conc
Resistant to Citric acidPass10% Conc
Resistant to Hydrogen peroxideFail
Resistant to Sulfuric acidFail96% Conc
Resistant to WaterPass<50°C, 100% Conc
Resistant to Zinc chloride, aqueousPass50% Conc

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Albis Plastics ANAmide Polyamide 6 PA F Black Unreinforced
Akro-Plastic Akromid® B3 GM 10/20 1 XL (4366) PA 6 Conditioned, 10/20% Glass/Mineral Filled
Akro-Plastic Akromid® B3 GK 30 black PA 6 Dry, 30% Glass Filled
Akro-Plastic Akromid® B3 GK 30 black PA 6 Conditioned, 30% Glass Filled
Akro-Plastic Akromid® B3 GF 30 4 RM-M black (3476) PA 6 Conditioned, 30% Glass Filled

PAKRO298 / 182885

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.