MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

SABIC SABIC® PP 2632/8 PP (Europe)
Categories: Polymer; Thermoplastic; Polypropylene (PP)

Material Notes: SABIC® PPcompound 2632/8 is a mineral filled modified polypropylene. Typical material properties include a very high flow and an excellent balance between impact and stiffness with the added advantage of a low shrinkage and CLTE. Typical applications include large automotive exterior parts such as bumpers. SABIC® PPcompound 2632/8 is a designated automotive grade. IMDS ID: 16486702

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.00 g/cc0.0361 lb/in³Injection molded sample ISO527-1A; ISO 1183
Filler Content 15 %15 %SABIC method
Linear Mold Shrinkage 0.0085 cm/cm0.0085 in/inInjection molded plaque 65x65x3.2mm; SABIC method
Melt Flow 18 g/10 min
@Load 2.16 kg,
Temperature 230 °C
18 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 15.0 MPa2180 psiISO 527/1A
Tensile Strength, Yield 18.0 MPa2610 psiISO 527/1A
Elongation at Break 100 %100 %ISO 527/1A
Tensile Modulus 1.50 GPa218 ksiISO 527/1A
Flexural Modulus 1.50 GPa218 ksiISO 178/1A
Izod Impact, Notched (ISO) NBNBISO 180/1A
 5.00 kJ/m²
@Temperature -20.0 °C
2.38 ft-lb/in²
@Temperature -4.00 °F
N.B.: No Break; ISO 180/1A
 10.0 kJ/m²
@Temperature 0.000 °C
4.76 ft-lb/in²
@Temperature 32.0 °F
N.B.: No Break; ISO 180/1A
 
Thermal PropertiesMetricEnglishComments
CTE, linear  70.0 µm/m-°C
@Temperature -30.0 - 30.0 °C
38.9 µin/in-°F
@Temperature -22.0 - 86.0 °F
ASTM D696
 80.0 µm/m-°C
@Temperature -30.0 - 100 °C
44.4 µin/in-°F
@Temperature -22.0 - 212 °F
ISO 11359-2
 90.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
50.0 µin/in-°F
@Temperature 73.4 - 176 °F
ASTM D696
Deflection Temperature at 0.46 MPa (66 psi) 100 °C212 °FISO 75

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABI11415 / 244882

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.