MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
DSM Biomedical Elasthane™ 75D Thermoplastic Polyether Polyurethane (TPU)
Categories: Polymer; Thermoplastic; Polyurethane, TP; Thermoplastic Polyurethane (TPUR), Polyether Grade

Material Notes: A high tensile strength, aromatic biomedical polymer with an exceptional combination of mechanical properties plus biological compatibility Elasthane™ TPU exhibits outstanding hydrolytic stability.

Widely Used This polyether-based polymer is designed to support long-term implantation and has been used in many commercially available medical devices including cardiovascular, neurostimulation and orthopedic implants.

Tailor Made Elasthane™ TPU can be enhanced with SME® technology to incorporate end groups that can address the needs of specific device applications. This eliminates the need for additional surface processing steps after the device component is fabricated.

Summary of Product Benefits

  • Excellent mechanical properties and abrasion resistance
  • Hydrolytically stable
  • Biocompatibile
  • Adaptable with SME® technology
  • Established FDA Master File

Information provided by DSM Biomedical.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.19 g/ccASTM D792
Linear Mold Shrinkage 0.016 in/in4 inch disk; ASTM D955
Linear Mold Shrinkage, Transverse 0.0050 - 0.0080 in/inFlame Bar; ASTM D955
Melt Flow 37 g/10 min
@Load 5.00 kg,
Temperature 224 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 75ASTM D2240
Tensile Strength, Ultimate 8734 psiASTM D1708
Elongation at Break 292 %ASTM D1708
Flexural Strength 10900 psiat 5% deflection; ASTM D790
Flexural Modulus, 1% Secant 289000 psiASTM D790
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 3.7
@Frequency 60 Hz
ASTM D150
Dielectric Strength 392 V/milASTM D149
 
Thermal PropertiesOriginal ValueComments
CTE, linear 86.4 µm/m-°C
@Temperature 20.0 °C
ASTM E-831
Vicat Softening Point 61.0 °CASTM D1525
 
Processing PropertiesOriginal ValueComments
Processing Temperature 194 - 221 °COptimum Extrusion Conditions
 
Descriptive Properties
ColorClear to Amber Pellets
CytotoxicityNon-cytotoxic
HemocompatibilityNon-hemolytic

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DSM Biomedical Elasthane™ 55D Thermoplastic Polyether Polyurethane (TPU)
DSM Biomedical Elasthane™ 80A Thermoplastic Polyether Polyurethane (TPU)
Covestro Desmopan® 453 Urethane Thermoplastic Elastomer
Covestro Texin® DP 7-1158 Urethane Thermoplastic Elastomer
BASF Elastollan® 1154 D KFFC TPUR

PBIOS003 / 79720

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.