MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Americhem Engineered Compounds ColorFast® ACR100 Polymethylmethacrylate
Categories: Polymer; Thermoplastic; Acrylic (PMMA)

Material Notes: High heat injection molding grade of PMMA

All information provided by LTL Color Compounders, Inc. LTL was acquired by Americhem in 2014.

Key Words: PMMA
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.19 g/ccASTM D792
Linear Mold Shrinkage 0.0020 - 0.0060 in/in0.125 in.; ASTM D955
Melt Flow 3.7 g/10 min
@Load 3.80 kg,
Temperature 230 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 93ASTM D785
Tensile Strength, Yield 10000 psi2.0 in/min; ASTM D638
Elongation at Break 6.0 %2.0 in/min; ASTM D638
Flexural Strength 15000 psi2.0 in/min; ASTM D790
Flexural Modulus 450000 psi2.0 in/min; ASTM D790
Izod Impact, Notched 0.400 ft-lb/in
@Temperature 22.8 °C
ASTM D256
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 216 °FUnannealed (0.250"); ASTM D648
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 410 - 450 °F
Middle Barrel Temperature 420 - 460 °F
Front Barrel Temperature 430 - 470 °F
Nozzle Temperature 420 - 460 °F
Melt Temperature 430 - 470 °F
Mold Temperature 150 - 190 °F
Drying Temperature 180 °F
Dry Time 3 - 4 hournominal; maximum drying time of 48 hours
Back Pressure 100 - 200 psi
Shot Size 40 - 60 %
Vent Depth 0.00100 - 0.00300 in
Screw Speed 40 - 70 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Americhem Engineered Compounds ColorFast® ACR100IM Polymethylmethacrylate, High Impact
Lucite International Lucite® 4F Acrylic Bead Resin
Trinseo Plexiglas® SG7 Acrylic
Isoflon PMMA Polymethyl-methacrylate
LG Chemical HI835HS PMMA, Impact Resistant Grade

PLTLC031 / 104416

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.