MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

LyondellBasell Petrothene NA980000 LDPE
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Low Density (LDPE); Low Density Polyethylene (LDPE), Film Grade

Material Notes: Petrothene NA980000 is a low density homopolymer resin selected for use in shrink packaging, bundling, pallet wrap and heavy-duty liner applications. NA980000 is also selected for use in blow molding squeeze bottles and other specialty applications. Excellent bubble stability, melt strength, impact and shrinkage are key attributes of NA980000. Applications: Agriculture Film, Bags & Pouches, Bottles and Vials, Bottles For Consumer Goods, Bottles for Industrial Use, Can Liners, Clear Containers, Film Wrap, Food Packaging Film, Heavy Duty Packaging, Liner Film, Opaque Containers, Shrink Film, Specialty Film, Textile Packaging Film.

Information provided by LyondellBasell.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Base Resin Density 0.920 g/cc0.0332 lb/in³ASTM D1505
Density 0.920 g/cc0.0332 lb/in³ASTM D1505
Melt Flow 0.25 g/10 min
@Load 2.16 kg,
Temperature 190 °C
0.25 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
Antiblock Level 0.000 ppm0.000 ppmLYB Method
Slip Level 0.000 ppm0.000 ppmLYB Method
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 4545ASTM D2240
Tensile Strength at Break 17.9 MPa2600 psiASTM D638
Tensile Strength, Yield 9.79 MPa1420 psiASTM D638
Film Elongation at Break, MD 310 %310 %ASTM D882
Film Elongation at Break, TD 430 %430 %ASTM D882
Elongation at Break 700 %700 %ASTM D638
Elongation at Yield 100 %100 %ASTM D638
Dart Drop Test 180 g0.397 lbF50; ASTM D1709
Film Tensile Strength at Break, MD 20.7 MPa3000 psiASTM D882
Film Tensile Strength at Break, TD 19.3 MPa2800 psiASTM D882
1% Secant Modulus, MD 207 MPa30000 psiASTM D882
1% Secant Modulus, TD 241 MPa35000 psiASTM D882
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 93.0 °C199 °FASTM D1525
 
Descriptive Properties
Processing MethodBlown Film, Extrusion Blow Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LyondellBasell Petrothene® NA960000 Low Density Polyethylene
Dow DOWLEX™ 2045G Linear Low Density Polyethylene
LyondellBasell Petrothene NA960183 LDPE
ExxonMobil LDPE LD 419.MV Low Density Polyethylene Resin
Chevron Phillips Marlex® 1122B Injection Molding Resin

PEQT8869 / 220503

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.