MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

1460 Alloy, 6 mm hot rolled sheet
Categories: Metal; Nonferrous Metal; Aluminum Alloy; Other Wrought Al Alloy

Material Notes: Russian Al-Li Alloy (Russian Federation Patent No. 1584414) used in aerospace cryogenic fuel tanks. Has low density and exhibits high strength, high elasticity, and high fatigue durability at both elevated (up to150°C) and cryogenic temperatures.

Key Words: Russian Aluminum-Lithium 1460 Alloy, Al-Li Alloys, Aluminium Alloy; Al1460
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.59 g/cc0.0936 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 540 MPa78300 psi
 760 MPa
@Temperature -253 °C
110000 psi
@Temperature -423 °F
Tensile Strength, Yield 470 MPa68200 psi
 560 MPa
@Temperature -253 °C
81200 psi
@Temperature -423 °F
Elongation at Break 7.5 %7.5 %
 12 %
@Temperature -253 °C
12 %
@Temperature -423 °F
Modulus of Elasticity 80.0 GPa11600 ksi
Shear Strength 319 MPa46300 psiCalculated
 446 MPa
@Temperature -253 °C
64700 psi
@Temperature -423 °F
Calculated
 
Thermal PropertiesMetricEnglishComments
CTE, linear 23.8 µm/m-°C
@Temperature 20.0 °C
13.2 µin/in-°F
@Temperature 68.0 °F
Estimated from similar Al-Li alloys
Specific Heat Capacity 0.860 J/g-°C0.206 BTU/lb-°FEstimated from similar Al-Li alloys
Thermal Conductivity 86.0 W/m-K597 BTU-in/hr-ft²-°FEstimated from similar Al-Li alloys

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
1460 Alloy, 20 mm plate
1460 Alloy, pressed profile
1201 Alloy 6 mm hot rolled sheet
1201 Alloy 20 mm plate
ASTM A36 Steel, plate

MA9A1460C / 9736

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.