MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Kotec Carbotex KG-15MRA Polycarbonate, 15% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, 20% Glass Filled

Material Notes: Features: Glass fiber 15% reinforced, Mold release, Translucent, Dimensional stability, Flame retardant, High rigidity
Applications: OA equipment, Communications, Precision parts, Machineries, E & E parts

Information provided by Kotec Corporation

Key Words: PC
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.30 g/ccASTM D792
Water Absorption 0.20 %
@Temperature 23.0 °C,
Time 86400 sec
ASTM D570
Linear Mold Shrinkage, Flow 0.0030 - 0.0050 cm/cmASTM D995
Linear Mold Shrinkage, Transverse 0.0030 - 0.0050 cm/cmASTM D995
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 98.0 MPaASTM D638
Elongation at Break 4.5 %ASTM D638
Flexural Strength 132 MPaASTM D790
Flexural Modulus 4410 MPaASTM D790
Izod Impact, Notched 78.0 J/m
@Temperature 23.0 °C
V-Notched 1/8"; ASTM D256
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+16 ohm-cmASTM D257
Dielectric Constant 3.2
@Frequency 1e+6 Hz
ASTM D150
Dielectric Strength 20.0 kV/mmASTM D149
Dissipation Factor 0.00080
@Frequency 1e+6 Hz
ASTM D150
Arc Resistance 110 secASTM D495
 
Thermal PropertiesOriginal ValueComments
Heat Distortion Temperature 143 °CASTM D648
Flammability, UL94 V-0
@Thickness 3.00 mm
 
Descriptive Properties
Light TransmittanceTranslucent3.0mm, ASTM D1003

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Ravago Manufacturing Americas Hylex® P1010G15 HB Polycarbonate, 15% Fiberglass Reinforced
Eurotec® Tecotek® PC43 GR10 BK002 PC, 10% glass fiber reinforced, black
Ravago Manufacturing Americas Hylex® P1310G10 HB Polycarbonate, 10% Fiberglass Reinforced, UV Stabilized
Ravago Manufacturing Americas Hylex® P1310G20 HB Polycarbonate, 20% Fiberglass Reinforced, UV Stabilized
E-Polymers TEKANATE™ G710 , 10% Glass Fiber Reinforced Poly Carbonate

PKOTEC030 / 93260

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.