MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Haysite SDL® H261 Polyester, Static Dissipative
Categories: Polymer; Thermoset; Polyester, TS

Material Notes: H261 is an advanced composite that combines high temperature resistant and high strength characteristics with static dissipative properties for use as wave and reflow solder pallets. SDL Grade H261 may be used as dedicated or adjustable flow solder carriers as well as surface mount pallets. Listed below are the expected performance properties of this material. H261 is available in sanded thicknesses from 3, 5, 6, 8, 10 and 12mm and in sheet sizes 36" x 72" and 48" x 96". Standard color is Black.

Information provided by Haysite

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.83 g/ccASTM D792
Water Absorption 0.16 %
@Time 86400 sec
ASTM D651
 
Mechanical PropertiesOriginal ValueComments
Hardness, Barcol 48ASTM D2583
Flexural Strength 6053 psi
@Temperature 150 °C
LW; ASTM D790
 6487 psi
@Temperature 150 °C
CW; ASTM D790
 27087 psi
@Temperature 25.0 °C
LW; ASTM D790
 33071 psi
@Temperature 25.0 °C
CW; ASTM D790
Flexural Modulus 589000 psi
@Temperature 150 °C
LW; ASTM D790
 661000 psi
@Temperature 150 °C
CW; ASTM D790
 1.513e+6 psi
@Temperature 25.0 °C
LW; ASTM D790
 1.658e+6 psi
@Temperature 25.0 °C
CW; ASTM D790
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1e+05 - 1.00e+9 ohm-cmASTM D257
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.5 µin/in-°FVSM 77110
Specific Heat Capacity 1.259 J/g-°CASTM E-1269-05
Thermal Conductivity 0.425 W/m-KASTM E-1925-06

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
IDI Composites E-206 Thermoset Polyester, Sheet

PHAY507 / 142463

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.